IBC battery aluminum paste, IBC battery and preparation method thereof

By using silver aluminum paste of aluminum powder, silver powder, boron powder, glass powder and organic additives in IBC batteries, it is directly printed and sintered on the passivation layer to form a positive gate line, which solves the problem of battery open circuit voltage reduction caused by laser grooves. , improves battery efficiency and filling quality.

CN116344096BActive Publication Date: 2024-11-05DAS SOLAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310333379.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-11-05
Estimated Expiration
2043-03-30

Smart Images

  • Figure CN116344096B_ABST
    Figure CN116344096B_ABST
Patent Text Reader

Abstract

The embodiment of the present invention provides an IBC battery aluminum paste, an IBC battery and a preparation method thereof, wherein the IBC battery aluminum paste provided by the embodiment of the present invention includes aluminum powder, silver powder, boron powder, glass powder, an organic adhesive and an organic additive. By adding silver powder to the aluminum paste, not only can the P+ emitter be replaced by aluminum powder, but also because the silver powder has a good burn-through property, after forming a passivation layer on the back of the battery silicon wafer, it is directly printed on the passivation layer area above the p+ doped area, and then sintered at high temperature, it can contact with the p+ doped area and form a positive electrode grid line, eliminating the step of secondary laser grooving, avoiding the damage of the passivation layer caused by the secondary laser grooving, and can improve the battery open circuit voltage, thereby solving the problem that the existing IBC battery silver aluminum paste needs to perform laser grooving on the P+ area before printing the positive electrode grid line, resulting in a decrease in the open circuit voltage value of the battery cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of crystalline silicon solar cell manufacturing, and in particular to an IBC battery aluminum paste, an IBC battery and a preparation method thereof. Background Art

[0002] The interdigitated back contact (IBC) battery is a new type of battery in which the contact electrodes of the P / N junction, substrate and emitter region are made in an interdigitated shape on the back of the battery. Its core technology is to prepare high-quality p-regions and n-regions arranged in an interdigitated shape on the back of the battery.

[0003] At present, before printing the grid lines, P-type IBC batteries need to perform laser grooving on the P+ region to facilitate printing of aluminum paste to form positive electrode grid lines. However, laser grooving not only increases the production process, but also damages the passivation layer, resulting in a decrease in the open circuit voltage value of the battery. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide an IBC battery aluminum paste, an IBC battery and a preparation method thereof, so as to solve the problem that before the existing IBC battery aluminum paste is printed into a positive electrode grid line, the P+ region needs to be laser grooved, resulting in a decrease in the open circuit voltage value of the battery cell.

[0005] In order to solve the above problems, the present invention is achieved through the following technical solutions:

[0006] The present invention provides an IBC battery aluminum paste, wherein the components constituting the aluminum paste include aluminum powder, silver powder, boron powder, glass powder, an organic binder and an organic additive.

[0007] Furthermore, in the IBC battery aluminum paste, the mass percentage of the organic additive is 0.6-1%; the mass percentage of the silver powder is 55-65%; the mass percentage of the aluminum powder is 5-10%; the mass percentage of the boron powder is 0.1-0.2%; the mass percentage of the organic binder is 21.8-37.8%; and the mass percentage of the glass powder is 1.5-2%.

[0008] Furthermore, in the IBC battery aluminum paste, the boron powder is boron aluminum alloy and / or elemental boron.

[0009] Furthermore, in the IBC battery aluminum paste, the organic additive includes two or more of fatty alcohol ether phosphate, aluminate coupling agent, silane coupling agent, zirconium aluminate coupling agent, lauryl phosphate, silicone oil, dibasic acid ester, and lauryl alcohol phosphate.

[0010] Furthermore, in the IBC battery aluminum paste, the silver powder includes 95-98% by mass of micron-spherical silver powder and 2-5% by mass of nano-spherical silver powder;

[0011] And / or the aluminum powder includes 85-90% by mass of micron spherical aluminum powder and 10-15% by mass of nano spherical aluminum powder.

[0012] Furthermore, in the IBC battery aluminum paste, the organic binder includes a high molecular polymer resin and an organic solvent;

[0013] The mass fraction of the high molecular weight polymer in the organic binder is 10 to 15%;

[0014] The mass fraction of the organic solvent in the organic binder is 85-90%.

[0015] Furthermore, in the IBC battery aluminum paste, the organic solvent is at least five of benzyl alcohol, diethyl phthalate, pineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve.

[0016] Furthermore, in the IBC battery aluminum paste, the glass powder is obtained by sintering and crushing 20-22% Bi2O3, 6-8% Al2O3, 10-12% SiO2, 5-29% ZnO, 15-20% Sb2O5, 5-8% TiO, 3-5% B2O3, and 15-20% TeO3 in mass percentage.

[0017] The present invention also proposes a method for preparing silver-aluminum paste for IBC batteries, which comprises:

[0018] mixing silver powder, aluminum powder, boron powder, an organic binder and glass powder to obtain a mixture;

[0019] After grinding the mixture, an organic additive is added to obtain an IBC battery silver-aluminum paste.

[0020] The present invention also proposes an IBC battery, wherein a plurality of positive electrode grid lines are attached to the back of the IBC battery, and the grid lines are prepared from the above-mentioned silver aluminum paste.

[0021] Compared with the prior art, the embodiments of the present invention have the following advantages:

[0022] In the embodiment of the present invention, the silver-aluminum paste for IBC batteries provided comprises aluminum powder, silver powder, boron powder, glass powder, organic adhesive and organic additive. By adding silver powder to the aluminum paste, not only can the P+ emitter be replaced by aluminum powder, but also because the silver powder has a good burn-through property, after forming a passivation layer on the back of the battery silicon wafer, it is directly printed on the passivation layer area above the p+ doped area, and then sintered at high temperature, it can contact with the p+ doped area and form a positive electrode grid line, eliminating the step of secondary laser grooving, avoiding the damage of the passivation layer caused by the secondary laser grooving, and can improve the battery open circuit voltage, thus solving the problem that the existing IBC battery silver-aluminum paste needs to perform laser grooving on the P+ area before printing the positive electrode grid line, resulting in a decrease in the open circuit voltage value of the battery cell.

[0023] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a flow chart of the method for preparing silver-aluminum paste for IBC batteries provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0025] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0026] The applicant of the present invention has found that the main component of the metallization printing paste of the current P-type IBC is aluminum paste, which will cause great metal complexation to the battery cell itself, increase the series resistance of the battery cell, reduce the electrical performance of the battery cell itself, and lead to low opening voltage, large series resistance, and poor filling, which can easily affect the efficiency of the battery cell itself.

[0027] In order to solve the above problems, an embodiment of the present invention provides an IBC battery silver-aluminum paste, wherein the components constituting the silver-aluminum paste include aluminum powder, silver powder, boron powder, glass powder, organic binder and organic additives.

[0028] The silver-aluminum paste for an IBC battery provided in an embodiment of the present invention is specifically a silver-aluminum paste for forming a positive grid line of a P-type IBC battery.

[0029] Among them, silver powder and aluminum powder are the main components, aluminum powder mainly replaces the P+ emitter of the battery, and silver paste has good thermal conductivity, electrical conductivity and burn-through performance. When the silver-aluminum paste is printed on the anti-reflection film layer on the back of the silicon wafer, the silicon nitride film and the silicon oxide film in the passivation layer can be burned through in sequence, and then contact with the p+ doped area to form a positive gate line, eliminating the step of secondary laser grooving and avoiding the damage of the passivation layer caused by the secondary laser grooving;

[0030] Among them, glass powder is an inorganic adhesive, which will melt into liquid under high temperature conditions and condense when cooled to play a bonding role; organic adhesives can ensure the overall bonding effect; organic additives can reduce the overall viscosity of the silver paste; and boron powder can diffuse into the silicon during high-temperature sintering for heavy doping, which is beneficial to improve the contact performance of the slurry and reduce the reaction contact area between aluminum and silicon; the above-mentioned silver-aluminum paste can quickly form a good alloy with silicon under lower sintering temperature conditions, reduce the contact resistivity between the front silver-aluminum fine grid and the battery, thereby improving the battery filling and battery efficiency.

[0031] Therefore, the silver-aluminum paste provided in the embodiment of the present invention has better contact with the battery cell itself, and the series resistance is smaller than that of traditional aluminum paste. The recombination rate and degree of recombination will also be greatly improved, and the opening voltage of the battery can be increased by 5 millivolts, thereby solving the problem that the existing P-type IBC battery needs to perform laser grooving on the P+ area when printing the positive electrode grid line, resulting in a decrease in the open circuit voltage value of the battery cell.

[0032] Optionally, in one embodiment, in the silver-aluminum paste, the mass percentage of organic additives is 0.6-1%; the mass percentage of silver powder is 55-65%; the mass percentage of aluminum powder is 5-10%; the mass percentage of boron powder is 0.1-0.2%; the mass percentage of organic binder is 21.8-37.8%; the mass percentage of glass powder is 1.5-2%. In the silver-aluminum paste provided by the embodiment of the present invention, the aluminum content is relatively low. When forming aluminum-silicon alloy, the proportion of aluminum in the aluminum-silicon alloy is relatively small, so during the cooling process, no excess aluminum will diffuse into the PN junction area to form a metal composite area.

[0033] For example, in the silver-aluminum paste, the mass fractions of the organic additive, silver powder, aluminum powder, boron powder, organic binder and glass powder are 0.6%, 65%, 5%, 0.1%, 27.3% and 2% respectively.

[0034] For example, in the silver-aluminum paste, the mass fractions of the organic additive, silver powder, aluminum powder, boron-aluminum alloy powder, organic binder and glass powder are 1%, 55%, 10%, 0.2%, 32.3% and 1.5% respectively.

[0035] For example, in the silver-aluminum paste, the mass fractions of the organic additive, silver powder, aluminum powder, boron-aluminum alloy powder, organic binder and glass powder are 1%, 65%, 10%, 0.2%, 21.8% and 2% respectively.

[0036] For example, in the silver-aluminum paste, the mass fractions of the organic additive, silver powder, aluminum powder, boron-aluminum alloy powder, organic binder and glass powder are 0.6%, 55%, 5%, 0.1%, 37.8% and 1.5%, respectively.

[0037] For example, in the silver-aluminum paste, the mass fractions of the organic additive, silver powder, aluminum powder, boron-aluminum alloy powder, organic binder and glass powder are 0.8%, 60%, 8%, 0.15%, 29.25% and 1.8%, respectively.

[0038] Optionally, in one embodiment, the boron powder includes micron-sized elemental boron. By adding the micron-sized elemental boron, the boron powder can quickly diffuse into the silicon for heavy doping during high-temperature sintering, which is beneficial to improving the contact performance of the slurry.

[0039] Optionally, in a specific embodiment, the boron powder is micron-grade boron powder with a boron powder purity of 3 9s.

[0040] Optionally, in another embodiment, the above includes boron aluminum alloy. By adding the micron-sized boron aluminum alloy powder, the silver aluminum paste can quickly form a good alloy with silicon under a lower sintering temperature condition, thereby reducing the contact resistivity between the front silver aluminum fine grid and the battery.

[0041] Optionally, in one embodiment, the silver powder includes 95-98% by mass of micron-sized spherical silver powder and 2-5% by mass of nano-sized spherical silver powder. Since there are gaps between the micron-sized silver powder and the silver powder, the nano-sized spherical silver powder can just fill and penetrate into the gaps between the micron-sized silver powder and the silver powder.

[0042] Optionally, in one embodiment, the aluminum powder includes 85-90% by mass of micron-sized spherical aluminum powder and 10-15% by mass of nano-sized spherical aluminum powder. Since there are gaps between the micron-sized aluminum powders, the nano-sized spherical aluminum powder can just fill and penetrate into the gaps between the micron-sized aluminum powders.

[0043] Optionally, in a specific embodiment, the aluminum powder includes micron-sized spherical aluminum powder with a purity of 3 9s, a mass fraction of 85-90%, and a D50 of 5-6 μm, and nano-sized spherical aluminum powder with a purity of 3 9s, a mass fraction of 10-15%, and a D50 of 7-9 nm.

[0044] Optionally, in one embodiment, the organic additive includes two or more of fatty alcohol ether phosphate, aluminate coupling agent, silane coupling agent, zirconium aluminate coupling agent, lauryl phosphate, silicone oil, dibasic acid ester, and lauryl alcohol phosphate mixture.

[0045] In the IBC battery silver-aluminum paste provided in the embodiment of the present invention, the above-mentioned organic binder includes a polymer resin and an organic solvent; wherein the polymer resin is dissolved in the organic solvent, so that the organic solvent can be used as an organic binder, that is, the paste plays a role of bonding powder after drying.

[0046] Optionally, in one embodiment, the mass fraction of the high molecular weight polymer in the organic binder is 10-15%; the mass fraction of the organic solvent in the organic binder is 85-90%.

[0047] Optionally, in one embodiment, the high molecular weight polymer is one or more of ethyl cellulose-N20, ethyl cellulose N-50, and ethyl cellulose-N100;

[0048] The organic solvent includes at least five of benzyl alcohol, diethyl phthalate, terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve.

[0049] Optionally, in one embodiment, the glass powder is obtained by sintering and crushing 20 to 22 parts of Bi2O3, 6 to 8 parts of Al2O3, 10 to 12 parts of SiO2, 5 to 29 parts of ZnO, 15 to 20 parts of Sb2O5, 5 to 8 parts of TiO, 3 to 5 parts of B2O3, and 15 to 20 parts of TeO3, by mass, and the D50 of the glass powder is 1.2 to 2 μm. If D50 is less than 1.2 μm, the glass activity is too high, and if D50 is greater than 2 μm, the glass activity is too low.

[0050] Among them, Bi2O3 is the main network structure, ZnO can break the network structure and promote glass crystallization, Al2O3 can adjust glass stability and increase viscosity; SiO2 is used for glass network formation, promoting glass stability and increasing glass melting point; Sb2O5 is used for clarification and uniformity of glass liquid; TiO2 is used for local crystallization, B2O3 is a network body, and TeO3 reduces the glass formation temperature. The D50 of glass powder is 1.5~2μm.

[0051] The present invention also provides a method for preparing silver-aluminum paste for IBC batteries, wherein: Figure 1 As shown, it includes steps 101 to 102:

[0052] Step 101, mixing silver powder, aluminum powder, boron powder, organic binder and glass powder to obtain a mixture;

[0053] Step 102: Grind the mixture, add an organic additive, and obtain silver-aluminum paste for IBC batteries.

[0054] In the above step 101, 55-65% of silver powder, 5-10% of aluminum powder, 0.1-0.2% of boron powder, 21.8-37.8% of organic binder, and 1.5-2% of glass powder are weighed and mixed, and dispersed by a disperser to obtain the above mixture.

[0055] Optionally, in one embodiment, in the above step 101, the organic adhesive and boron powder are first mixed and dispersed using a disperser, and then silver powder, aluminum powder and glass powder are added, dispersed again using a disperser, and then ground to obtain the above mixture.

[0056] In the above step 102, the above mixture is ground and then an organic additive accounting for 0.6-1% of the total mass of the raw materials is added. After high-speed dispersion, a positive electrode grid line that contacts the P+ area on the back of the IBC battery is obtained without laser grooving, thereby avoiding damage to the passivation layer caused by laser grooving.

[0057] In the embodiment of the present invention, by adding silver powder to the aluminum paste, not only can the P+ emitter be replaced by aluminum powder, but also because the silver powder has a good burn-through property, after forming a passivation layer on the back of the battery silicon wafer, it is directly printed on the passivation layer area above the p+ doped area, and then subjected to high-temperature sintering, it can contact with the p+ doped area and form a positive electrode grid line, eliminating the step of secondary laser grooving, avoiding damage to the passivation layer caused by the secondary laser grooving, and being able to improve the battery open circuit voltage. Therefore, the problem that the existing IBC battery silver aluminum paste needs to perform laser grooving on the P+ area before printing the positive electrode grid line, resulting in a decrease in the open circuit voltage value of the battery cell is solved.

[0058] Optionally, in the preparation method provided in the embodiment of the present invention, the boron powder is micron-sized boron aluminum alloy and / or micron-sized elemental boron. Micron-sized boron aluminum alloy and micron-sized elemental boron have the characteristics of high tap density, low oxygen content and high activity. By adding the micron-sized boron aluminum alloy powder and / or micron-sized elemental boron, the silver aluminum paste can quickly form a good alloy with silicon under low sintering temperature conditions, thereby reducing the contact resistivity between the front silver aluminum fine grid and the battery.

[0059] Optionally, in the preparation method provided in an embodiment of the present invention, the organic additive includes two or more of fatty alcohol ether phosphate, aluminate coupling agent, silane coupling agent, zirconium aluminate coupling agent, lauryl phosphate, silicone oil, dibasic acid ester, and lauryl alcohol phosphate.

[0060] Optionally, in the preparation method provided in the embodiment of the present invention, the silver powder includes 95-98% by mass of micron spherical silver powder and 2-5% by mass of nano spherical silver powder.

[0061] Optionally, in the preparation method provided in the embodiment of the present invention, the aluminum powder includes 85-90% by mass of micron spherical aluminum powder and 10-15% by mass of nano spherical aluminum powder.

[0062] Optionally, in the preparation method provided in the embodiment of the present invention, the organic binder comprises a high molecular polymer resin and an organic solvent;

[0063] The mass fraction of the high molecular weight polymer in the organic binder is 10 to 15%;

[0064] The mass fraction of the organic solvent in the organic binder is 85-90%.

[0065] Optionally, in the preparation method provided in an embodiment of the present invention, the organic solvent is at least five of benzyl alcohol, diethyl phthalate, terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve.

[0066] Optionally, in the preparation method provided in an embodiment of the present invention, the glass powder is obtained by sintering and crushing 20-22% Bi2O3, 6-8% Al2O3, 10-12% SiO2, 5-29% ZnO, 15-20% Sb2O5, 5-8% TiO, 3-5% B2O3, and 15-20% TeO3 in mass percentage.

[0067] The present invention also proposes an IBC battery, wherein a plurality of positive electrode grid lines are attached to the back of the IBC battery, and the grid lines are prepared from the above-mentioned silver aluminum paste.

[0068] The steps of manufacturing an IBC battery using the silver-aluminum paste provided in the embodiment of the present invention are as follows:

[0069] (1) After forming an ultra-thin silicon oxide layer and a polysilicon layer on the back of a P-type silicon wafer, phosphorus is doped into the back polysilicon layer;

[0070] (2) forming interdigitated n+ doped regions and p+ doped regions by laser grooving; then performing double-sided atomic layer deposition (ALD) to form an aluminum oxide film, and a silicon nitride film on the front and back sides to form a passivation layer;

[0071] (3) screen printing is performed on the coated silicon wafer, and silver-aluminum paste is printed on the passivation layer directly opposite to the p+ doped area, and silver paste is printed on the passivation layer directly opposite to the n+ doped area;

[0072] (4) The printed silicon wafer is sintered at high temperature to produce a P-type IBC battery.

[0073] The present invention is described in detail below by way of examples.

[0074] Example 1

[0075] (1) Providing silver-aluminum paste a1: In parts by mass, the silver-aluminum paste a1 for IBC batteries is composed of 0.6 parts of organic additives, 65 parts of silver powder, 5 parts of aluminum powder, 0.1 parts of boron powder, 27.3 parts of organic binder and 2 parts of glass powder;

[0076] Among them, the above-mentioned organic additive is a silane coupling agent; the silver powder includes micron-grade spherical silver powder with a purity of 3 nines and a mass fraction of 95% and nano-grade spherical silver powder with a purity of 3 nines and a mass fraction of 5%; the aluminum powder includes micron-grade spherical aluminum powder with a purity of 3 nines and a mass fraction of 85% and a D50 of 5 to 6 μm, and nano-spherical aluminum powder with a purity of 3 nines and a mass fraction of 15% and a D50 of 7 to 9 nm; the organic binder includes ethyl cellulose-N100 with a mass fraction of 88% and an organic solvent with a mass fraction of 12%, and the organic solvent is composed of benzyl alcohol, diethyl phthalate, pineneol, tributyl citrate, Span 85 and alcohol ester twelve.

[0077] (2) After forming a silicon oxide layer and a polysilicon layer on the back of the P-type silicon wafer, phosphorus is doped into the back polysilicon layer;

[0078] (3) laser grooving the back side of the phosphorus-doped P-type silicon wafer to form interdigitated n+ doped regions and p+ doped regions, and removing the front polysilicon layer;

[0079] (4) After removing the front polysilicon layer and sequentially forming a double-sided aluminum oxide layer, a front silicon nitride layer, and a back silicon nitride layer, the above-mentioned silver aluminum paste a1 is printed on the back silicon nitride layer facing the p+ doped region, and the silver paste is printed on the back silicon nitride layer facing the n+ doped region;

[0080] (5) The silicon wafer is sintered at a high temperature in a sintering furnace, with a peak sintering temperature of 772° C., to produce an IBC battery.

[0081] After sintering, the electrical properties tested were: open circuit voltage of 718.2 mV and photoelectric conversion efficiency of 25.145%.

[0082] Example 2

[0083] (1) Providing silver-aluminum paste a2: In parts by mass, the IBC battery silver-aluminum paste a2 is composed of 1 part of organic additive, 55 parts of silver powder, 10 parts of aluminum powder, 0.2 parts of boron powder, 32.3 parts of organic binder and 1.5 parts of glass powder;

[0084] Among them, the above-mentioned organic additive is a silane coupling agent; the silver powder includes micron-grade spherical silver powder with a purity of 3 nines and a mass fraction of 95% and nano-grade spherical silver powder with a purity of 3 nines and a mass fraction of 5%; the aluminum powder includes micron-grade spherical aluminum powder with a purity of 3 nines and a mass fraction of 85% and a D50 of 5 to 6 μm, and nano-spherical aluminum powder with a purity of 3 nines and a mass fraction of 15% and a D50 of 7 to 9 nm; the organic binder includes ethyl cellulose-N100 with a mass fraction of 88% and an organic solvent with a mass fraction of 12%, and the organic solvent is composed of benzyl alcohol, diethyl phthalate, pineneol, tributyl citrate, Span 85 and alcohol ester twelve.

[0085] (2) After forming a silicon oxide layer and a polysilicon layer on the back of the P-type silicon wafer, phosphorus is doped into the back polysilicon layer;

[0086] (3) laser grooving the back side of the phosphorus-doped P-type silicon wafer to form interdigitated n+ doped regions and p+ doped regions, and removing the front polysilicon layer;

[0087] (4) after removing the front polysilicon layer and sequentially forming a double-sided aluminum oxide layer, a front silicon nitride layer, and a back silicon nitride layer, the silver aluminum paste is printed on the back silicon nitride layer facing the p+ doped region, and the silver paste is printed on the back silicon nitride layer facing the n+ doped region;

[0088] (5) The silicon wafer is sintered at a high temperature in a sintering furnace, with a peak sintering temperature of 776° C., to produce an IBC battery.

[0089] After sintering, the electrical properties tested were: open circuit voltage of 719.1 mV and photoelectric conversion efficiency of 25.153%.

[0090] Example 3

[0091] (1) Providing silver-aluminum paste a3: In parts by mass, the silver-aluminum paste a3 for IBC batteries is composed of 1 part of an organic additive, 65 parts of silver powder, 10 parts of aluminum powder, 0.2 parts of boron powder, 21.8 parts of an organic binder and 2 parts of glass powder;

[0092] Among them, the above-mentioned organic additive is a silane coupling agent; the silver powder includes micron-grade spherical silver powder with a purity of 3 nines and a mass fraction of 95% and nano-grade spherical silver powder with a purity of 3 nines and a mass fraction of 5%; the aluminum powder includes micron-grade spherical aluminum powder with a purity of 3 nines and a mass fraction of 85% and a D50 of 5 to 6 μm, and nano-spherical aluminum powder with a purity of 3 nines and a mass fraction of 15% and a D50 of 7 to 9 nm; the organic binder includes ethyl cellulose-N100 with a mass fraction of 88% and an organic solvent with a mass fraction of 12%, and the organic solvent is composed of benzyl alcohol, diethyl phthalate, pineneol, tributyl citrate, Span 85 and alcohol ester twelve.

[0093] (2) After forming a silicon oxide layer and a polysilicon layer on the back of the P-type silicon wafer, phosphorus is doped into the back polysilicon layer;

[0094] (3) laser grooving the back side of the phosphorus-doped P-type silicon wafer to form interdigitated n+ doped regions and p+ doped regions, and removing the front polysilicon layer;

[0095] (4) After removing the front polysilicon layer and sequentially forming a double-sided aluminum oxide layer, a front silicon nitride layer, and a back silicon nitride layer, the above-mentioned silver aluminum paste a3 is printed on the back silicon nitride layer facing the p+ doped region, and the silver paste is printed on the back silicon nitride layer facing the n+ doped region;

[0096] (5) The silicon wafer is sintered at a high temperature in a sintering furnace, with the peak sintering temperature being 774° C., to produce an IBC battery.

[0097] After sintering, the electrical properties tested were: open circuit voltage of 720.5 mV and photoelectric conversion efficiency of 25.172%.

[0098] Example 4

[0099] (1) Providing silver-aluminum paste a4: In parts by mass, the silver-aluminum paste a4 for IBC batteries is composed of 0.6 parts of organic additives, 55 parts of silver powder, 5 parts of aluminum powder, 0.1 parts of boron powder, 37.8 parts of organic binder and 1.5 parts of glass powder;

[0100] Among them, the above-mentioned organic additive is a silane coupling agent; the silver powder includes micron-grade spherical silver powder with a purity of 3 nines and a mass fraction of 95% and nano-grade spherical silver powder with a purity of 3 nines and a mass fraction of 5%; the aluminum powder includes micron-grade spherical aluminum powder with a purity of 3 nines and a mass fraction of 85% and a D50 of 5 to 6 μm, and nano-spherical aluminum powder with a purity of 3 nines and a mass fraction of 15% and a D50 of 7 to 9 nm; the organic binder includes ethyl cellulose-N100 with a mass fraction of 88% and an organic solvent with a mass fraction of 12%, and the organic solvent is composed of benzyl alcohol, diethyl phthalate, pineneol, tributyl citrate, Span 85 and alcohol ester twelve.

[0101] (2) After forming a silicon oxide layer and a polysilicon layer on the back of the P-type silicon wafer, phosphorus is doped into the back polysilicon layer;

[0102] (3) laser grooving the back side of the phosphorus-doped P-type silicon wafer to form interdigitated n+ doped regions and p+ doped regions, and removing the front polysilicon layer;

[0103] (4) After removing the front polysilicon layer and sequentially forming a double-sided aluminum oxide layer, a front silicon nitride layer, and a back silicon nitride layer, the above-mentioned silver aluminum paste a4 is printed on the back silicon nitride layer facing the p+ doped region, and silver paste is printed on the back silicon nitride layer facing the n+ doped region;

[0104] (5) The silicon wafer is sintered at a high temperature in a sintering furnace, with a peak sintering temperature of 776° C., to produce an IBC battery.

[0105] After sintering, the electrical properties tested were: open circuit voltage of 721.2 mV and photoelectric conversion efficiency of 25.189%.

[0106] Example 5

[0107] (1) Providing silver-aluminum paste a5: In parts by mass, the IBC battery silver-aluminum paste a5 is composed of 0.8 parts of organic additives, 60 parts of silver powder, 8 parts of aluminum powder, 0.15 parts of boron powder, 29.25 parts of organic binder and 1.8 parts of glass powder;

[0108] Among them, the above-mentioned organic additive is a silane coupling agent; the silver powder includes micron-grade spherical silver powder with a purity of 3 nines and a mass fraction of 95% and nano-grade spherical silver powder with a purity of 3 nines and a mass fraction of 5%; the aluminum powder includes micron-grade spherical aluminum powder with a purity of 3 nines and a mass fraction of 85% and a D50 of 5 to 6 μm, and nano-spherical aluminum powder with a purity of 3 nines and a mass fraction of 15% and a D50 of 7 to 9 nm; the organic binder includes ethyl cellulose-N100 with a mass fraction of 88% and an organic solvent with a mass fraction of 12%, and the organic solvent is composed of benzyl alcohol, diethyl phthalate, pineneol, tributyl citrate, Span 85 and alcohol ester twelve.

[0109] (2) After forming a silicon oxide layer and a polysilicon layer on the back of the P-type silicon wafer, phosphorus is doped into the back polysilicon layer;

[0110] (3) laser grooving the back side of the phosphorus-doped P-type silicon wafer to form interdigitated n+ doped regions and p+ doped regions, and removing the front polysilicon layer;

[0111] (4) After removing the front polysilicon layer and sequentially forming a double-sided aluminum oxide layer, a front silicon nitride layer, and a back silicon nitride layer, the above-mentioned silver aluminum paste a5 is printed on the back silicon nitride layer facing the p+ doped region, and the silver paste is printed on the back silicon nitride layer facing the n+ doped region;

[0112] (5) The silicon wafer is sintered at a high temperature in a sintering furnace, with a peak sintering temperature of 776° C., to produce an IBC battery.

[0113] After sintering, the electrical properties tested were: open circuit voltage of 721.9 mV and photoelectric conversion efficiency of 25.201%.

[0114] Comparative Example 1

[0115] (1) Providing silver-aluminum paste b1: In parts by mass, the silver-aluminum paste b1 for IBC batteries is composed of 0.8 parts of organic additives, 68 parts of aluminum powder, 0.15 parts of boron powder, 29.25 parts of organic binder and 1.8 parts of glass powder;

[0116] Among them, the above-mentioned organic additive is a silane coupling agent; the aluminum powder includes micron-sized spherical aluminum powder with a purity of 3 9s, a mass fraction of 85%, and a D50 of 5 to 6 μm, and nano-spherical aluminum powder with a purity of 3 9s, a mass fraction of 15%, and a D50 of 7 to 9 nm; the organic binder includes ethyl cellulose-N100 with a mass fraction of 88% and an organic solvent with a mass fraction of 12%, and the organic solvent is composed of benzyl alcohol, diethyl phthalate, pine alcohol, tributyl citrate, Span 85 and alcohol ester twelve.

[0117] (2) After forming a silicon oxide layer and a polysilicon layer on the back of the P-type silicon wafer, phosphorus is doped into the back polysilicon layer;

[0118] (3) laser grooving the back side of the phosphorus-doped P-type silicon wafer to form interdigitated n+ doped regions and p+ doped regions, and removing the front polysilicon layer;

[0119] (4) After removing the front polysilicon layer and sequentially forming a double-sided aluminum oxide layer, a front silicon nitride layer, and a back silicon nitride layer, the p+ doped region is laser grooved, and the above-mentioned silver aluminum paste b1 is printed in the laser groove that is conductive to the p+ doped region, and the silver paste is printed on the back silicon nitride that is opposite to the n+ doped region;

[0120] (5) The silicon wafer is sintered at a high temperature in a sintering furnace, with a peak sintering temperature of 772° C., to produce an IBC battery.

[0121] After sintering, the electrical properties tested were: open circuit voltage of 712.8 mV and photoelectric conversion efficiency of 24.891%.

[0122] By comparing Examples 1 to 5 with Comparative Example 1, it can be seen that by forming the P+ emitter using aluminum paste doped with silver, the positive electrode grid line can be formed without laser grooving, and the recombination rate and degree of the battery will also be greatly improved. The efficiency of the battery is increased by 0.254%, and the start-up voltage is increased by 6mv.

[0123] To sum up, in this embodiment, by adding silver powder to the aluminum paste, not only can the P+ emitter be replaced by aluminum powder, but also because the silver powder has good burn-through properties, after the passivation layer is formed on the back of the battery silicon wafer, it is directly printed on the passivation layer area above the p+ doped area, and then subjected to high-temperature sintering, it can contact the p+ doped area and form a positive electrode grid line, thereby eliminating the step of secondary laser grooving, thus avoiding damage to the passivation layer caused by the secondary laser grooving, and being able to improve the battery open circuit voltage. Therefore, the problem that the existing IBC battery silver aluminum paste needs to perform laser grooving on the P+ area before printing the positive electrode grid line, resulting in a decrease in the open circuit voltage value of the battery cell is solved.

[0124] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they are aware of the basic creative concept. Therefore, the claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present invention.

[0125] The above is a detailed introduction to an IBC battery aluminum paste, an IBC battery and a preparation method thereof provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as a limitation on the present invention.

Claims

1. Application of IBC battery silver aluminum paste in IBC battery, characterized in that: The components constituting the silver-aluminum paste include aluminum powder, silver powder, boron powder, glass powder, organic binder and organic additives; The mass percentage of the organic additive is 0.6-1%; the mass percentage of the silver powder is 55-65%; the mass percentage of the aluminum powder is 5-10%; the mass percentage of the boron powder is 0.1-0.2%; the mass percentage of the organic binder is 21.8-37.8%; the mass percentage of the glass powder is 1.5-2%; The silver powder includes 95-98% by mass of micron-spherical silver powder and 2-5% by mass of nano-spherical silver powder; The aluminum powder includes 85-90% by mass of micron spherical aluminum powder and 10-15% by mass of nano spherical aluminum powder; The silver aluminum paste is used to prepare the IBC battery by the following steps: After forming an ultra-thin silicon oxide layer and a polysilicon layer on the back of the P-type silicon wafer, phosphorus is doped into the back polysilicon layer; Laser grooving is used to form interdigitated n+ doped regions and p+ doped regions; double-sided atomic layer deposition is then performed to form an aluminum oxide film, and a silicon nitride film is formed on the front and back sides to form a passivation layer; Screen printing is performed on the coated silicon wafer, the silver-aluminum paste is printed on the passivation layer directly opposite to the p+ doped region, and the silver paste is printed on the passivation layer directly opposite to the n+ doped region; The printed silicon wafer is sintered at high temperature to produce a P-type IBC battery; A plurality of positive grid lines are attached to the back of the IBC battery, and the grid lines are prepared from the silver-aluminum paste.

2. The use of the IBC battery silver aluminum paste in an IBC battery according to claim 1, characterized in that: The boron powder includes micron-sized elemental boron.

3. The use of the IBC battery silver aluminum paste in an IBC battery according to claim 1, characterized in that: The organic additives include two or more of fatty alcohol ether phosphate, aluminate coupling agent, silane coupling agent, zirconium aluminate coupling agent, lauryl phosphate, silicone oil, dibasic acid ester, and lauryl alcohol phosphate.

4. The use of the IBC battery silver aluminum paste in an IBC battery according to claim 1, characterized in that: The organic binder includes a high molecular polymer resin and an organic solvent; The mass fraction of the high molecular weight polymer in the organic binder is 10-15%; The mass fraction of the organic solvent in the organic binder is 85-90%.

5. The use of the IBC battery silver aluminum paste in an IBC battery according to claim 1, characterized in that: The organic solvent is at least five of benzyl alcohol, diethyl phthalate, terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve.

6. The use of the IBC battery silver aluminum paste in an IBC battery according to claim 1, characterized in that: The glass powder is obtained by sintering and crushing 20-22% of Bi2O3, 6-8% of Al2O3, 10-12% of SiO2, 5-29% of ZnO, 15-20% of Sb2O5, 5-8% of TiO, 3-5% of B2O3 and 15-20% of TeO3 in mass percentage.

7. The use of the IBC battery silver aluminum paste in an IBC battery according to claim 1, characterized in that: include: mixing silver powder, aluminum powder, boron powder, an organic binder and glass powder to obtain a mixture; After grinding the mixture, an organic additive is added to obtain an IBC battery silver-aluminum paste.

8. An IBC battery, characterized in that: A plurality of positive grid lines are attached to the back of the IBC battery, and the grid lines are prepared by the silver-aluminum paste described in any one of claims 1 to 7; The silver aluminum paste is used to prepare the IBC battery by the following steps: After forming an ultra-thin silicon oxide layer and a polysilicon layer on the back of the P-type silicon wafer, phosphorus is doped into the back polysilicon layer; Laser grooving is used to form interdigitated n+ doped regions and p+ doped regions; double-sided atomic layer deposition is then performed to form an aluminum oxide film, and a silicon nitride film is formed on the front and back sides to form a passivation layer; Screen printing is performed on the coated silicon wafer, the silver-aluminum paste is printed on the passivation layer directly opposite to the p+ doped region, and the silver paste is printed on the passivation layer directly opposite to the n+ doped region; The printed silicon wafer is sintered at high temperature to produce a P-type IBC battery.