P-type Hessler-like thermoelectric materials and their preparation methods
By doping Fe and Cu atoms at the interstitial sites of Half-Heusler alloys, TiFexCu2x-1Sb thermoelectric materials were prepared, solving the problem of poor tunability of thermoelectric properties in alloys with non-18 valence electrons. This achieved efficient thermoelectric conversion and unique physical properties, broadening the application of the Heusler alloy system.
Patent Information
- Application Number
- CN202310264735.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-03-20
AI Technical Summary
The poor thermoelectric property tunability and low thermal conductivity of existing Half-Heusler alloys with non-18 valence electrons limit their development, resulting in low thermoelectric conversion efficiency.
TiFexCu2x-1Sb thermoelectric material was prepared by doping Fe and Cu atoms at interstitial sites using high-energy ball milling and spark plasma sintering. The atomic content was adjusted by utilizing the valence bond balance rule to form a stable Hessler-like structure.
It achieves highly efficient thermoelectric conversion performance. The material has a high power factor and low thermal conductivity at a temperature of 973K, with a zT value of 0.75. It also possesses unique physical properties, such as non-Fermi liquid metal characteristics, and has potential applications in thermoelectricity, magnetism, and superconductivity.
Smart Images

Figure CN116347970B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of thermoelectric materials technology, specifically to a P-type Hessler-like thermoelectric material and its preparation method. Background Technology
[0002] With rapid societal development and rising living standards, the demand for energy, especially electricity, is also increasing. Unlike primary energy sources such as oil and coal, electricity, as a secondary energy source, cannot be directly extracted. The process of obtaining electricity inevitably involves significant energy loss during energy conversion, much of which is wasted as heat. However, heat, despite its widespread existence, is rarely utilized. The energy problem remains a pressing issue, and seeking different sustainable and green transformation pathways is a goal that requires continuous effort.
[0003] Thermoelectric materials are materials that enable the direct conversion between thermal energy and electrical energy. Their fundamental theory lies in the Seebeck and Peltier effects, and they possess advantages such as small size, light weight, no pollution, no noise, and high reliability. Thermoelectric materials can utilize heat energy generated from various sources, such as industrial waste heat and automobile exhaust heat, to produce the electrical energy needed by people. This energy reuse process improves energy efficiency. Thermoelectric materials encompass numerous material systems, and materials with excellent thermoelectric properties and thermal stability can be found for different temperature application scenarios.
[0004] In thermoelectric material systems, the dimensionless thermoelectric figure of merit zT can be used to evaluate the thermoelectric performance of a material. The magnitude of zT determines the efficiency of the thermoelectric material in cooling and power generation during application. Typically, zT = S 2 σT / κ, where S, σ, κ, and T are the Seebeck coefficient, electrical conductivity, thermal conductivity, and absolute temperature of the environment, respectively.
[0005] Half-Heusler (HH) alloys are a class of medium-to-high temperature thermoelectric materials, exhibiting good thermal stability and mechanical properties at high temperatures. They are generally classified by the number of valence electrons. HH alloys with 18 valence electrons often exhibit semiconductor physical properties, displaying high power factors and high thermal conductivity. Those with non-18 valence electrons, such as 17, 19, and 22, are less studied due to their lower thermoelectric performance, sometimes even exhibiting metallic-like thermoelectric properties. These non-18 valence electron HH alloys often exist stably as intrinsic defects and possess low lattice thermal conductivity. However, the limited variety and tunability of these intrinsic defects restrict their development, hindering the effective utilization of their inherent low thermal conductivity. Summary of the Invention
[0006] The purpose of this invention is to provide a P-type Hessler-like thermoelectric material and its preparation method. By doping at interstitial positions and adjusting the atomic content, the aforementioned problems of poor tunability and low thermoelectric performance of non-18-valent electron number HH are solved. It also inherits the advantages of low lattice thermal conductivity of this type of non-18-valent electron number HH.
[0007] The objective of this invention can be achieved through the following technical solution: a P-type Hessler-like thermoelectric material, with the chemical formula: TiFe x Cu 2x-1 Sb, where x takes values in the range of 0.67 ≤ x ≤ 1.
[0008] Preferably, in the chemical formula, x = 0.7, 0.75, or 0.8.
[0009] More preferably, the electrical conductivity of the thermoelectric material is between 46,000 and 105,000 S / m, the Seebeck coefficient is between 10⁴ and 194 μV / K, and the power factor is between 10.3 and 20.8 μW / (cm·K). 2 The thermal conductivity is between 2.6 and 5.7 W / (m·K), and the zT value is between 0.07 and 0.75.
[0010] More preferably, in the chemical formula, x = 0.7, and the highest power factor at 973 K is 20.8 μW / (cm·K). 2 The lowest thermal conductivity is 2.6 W / (m·K), and the highest zT is 0.75.
[0011] A method for preparing the above-mentioned P-type Hessler-structure thermoelectric material, using elemental Ti particles, Fe sheets, Cu particles, and Sb particles as raw materials, and employing high-energy ball milling (HEBM) and spark plasma sintering (SPS) methods.
[0012] Preferably, the preparation method of the P-type Hessler-like thermoelectric material includes the following steps:
[0013] a. Calculation: Based on the stoichiometric ratio of 1:x:(2x-1):1, calculate the mass of each element corresponding to a specific x value.
[0014] b. Sample preparation: Weigh the elemental Ti particles, Fe flakes, Cu particles, and Sb particles according to the mass calculated in step a, and place the weighed raw materials in a stainless steel ball mill jar;
[0015] c. Alloying: The ball mill jar from step b is placed in a high-energy ball mill and subjected to continuous ball milling and material collision for a long time to obtain mixed powder;
[0016] d. Sintering: Weigh a certain amount of the mixed powder obtained in step c into a graphite mold, then place the mold into a spark plasma sintering device, evacuate it and apply a certain pressure to start sintering, and finally hold it at a certain temperature for a period of time, then release the pressure and let it cool naturally to room temperature to obtain the thermoelectric material.
[0017] More preferably, the total amount of raw materials weighed in step a is generally 0.04 mol. The required mass of each element can be calculated by using the formula m = n × M (n: the molar amount of a certain element under a specific composition, m: the required mass, M: atomic molar mass) and the stoichiometric ratio of the corresponding composition.
[0018] More preferably, in step b, the elemental Ti particles, Fe flakes, Cu particles, and Sb particles are weighed in an argon glove box according to the mass calculated in step a.
[0019] More preferably, the mixed powder obtained in step c is stored in an argon glove box.
[0020] More preferably, the ball milling time set in step c is 28-32 hours to ensure that the raw materials are fully mixed and completely ball-milled into powder.
[0021] More preferably, the ball milling time set in step c is 30 hours.
[0022] More preferably, in step d, the sintering gas pressure is 58-62 MPa and the applied pressure is 6-6.5 kN, the temperature is raised to 650-750℃ at a sintering rate of 30-50℃ / min, and the holding time is 10-15 min.
[0023] More preferably, in step d, the sintering gas pressure is 60 MPa and the applied pressure is 6.3 kN. The temperature is raised to 700°C in 20 minutes at a sintering rate of 30-50°C / min, and the holding time is 10-15 minutes.
[0024] More preferably, the graphite mold in step d has a diameter of 12.7 mm, and after sintering, a circular thermoelectric material with a thickness of 1-2 mm is obtained.
[0025] Preferably, the purity of the elemental Ti particles, Fe flakes, Cu particles, and Sb particles are 99.6%, 99.99%, 99.99%, and 99.999%, respectively.
[0026] This invention first constructs a vacancy-filled HH framework. Typically, the stoichiometric ratio of the three different atoms in this type of Hessler alloy deviates from 1:1:1. However, this invention selects a NaCl-type crystal structure composed of Ti and Sb as the filling framework. Then, a certain amount of atoms are randomly filled into the tetrahedral interstitial positions of this face-centered cubic structure. To achieve this, the invention made the following attempts:
[0027] From the perspective of 17-valent electrons (HH), the initial attempt was to fill the interstitial positions with only Fe atoms. This resulted in the formation of a stable pure phase, but this single-filling method suffers from the aforementioned problems: it can only form a stable pure phase under specific compositions and its performance is relatively low. This invention plans to further fill the interstitial positions with another type of atom. Since the composition of quaternary Hessler alloys with two different atoms as interstitial fillers exhibits significant randomness and unknown phase stability, this invention uses the valence bond balance rule for the study of this type of Hessler alloy system. According to the valence bond balance rule, each bonded atom generally exhibits a full-shell valence bond structure to achieve a stable state. As one of the filling atoms, the Fe atom will gain electrons after reaching a stable state. Therefore, to ensure the conservation of electrons in the entire system, this invention selected Cu as another filling atom. Furthermore, Cu is cheaper than other transition metals, and Fe and Cu atoms with similar atomic radii are easier to successfully dope at interstitial positions. According to the valence bond equilibrium rule, there is a series of adjustable ratios for Fe and Cu atoms filling interstitial positions, with the ratio being Fe:Cu = x:(2x-1), and the chemical formula being TiFe. x Cu 2x-1 Sb, where 0.67 ≤ x ≤ 1. This invention has discovered that filling atoms in this ratio can form a stable phase, such as... Figure 1 As shown, all synthesized samples are pure phases with a Hessler-like structure.
[0028] To achieve the above-mentioned objectives, this invention employs a mechanical alloying method in the alloy preparation process. This method not only avoids the problem of Sb volatilization but also reduces preparation time. The mechanically alloyed powder is then stabilized through rapid sintering, ensuring a shorter alloy preparation process while retaining more grain boundaries to further reduce thermal conductivity.
[0029] The concepts involved in this invention may not be applicable only to the system mentioned in the present invention. Combining different elements may lead to the exploration of more high-performance HH thermoelectric materials, thereby broadening the Hessler alloy system and accelerating its development and application.
[0030] Compared with the prior art, the present invention has the following advantages:
[0031] 1. The samples tested in this invention were all synthesized using high-energy ball milling (HEBM) and spark plasma sintering (SPS), a process that is convenient to operate and has a short preparation time.
[0032] 2. This invention is not a traditional HH compound conforming to stoichiometry, but a novel vacancy-filling Hessler-like alloy.
[0033] 3. In filling the interstitial positions with Fe and Cu atoms, this invention explored the valence bond balance rule and found a component with better performance within a certain composition range.
[0034] 4. The thermoelectric material prepared by this invention is not a semiconductor material, but an alloy with non-Fermi liquid metal characteristics, and has thermoelectric properties comparable to some semiconductor thermoelectric materials.
[0035] 5. The material of this invention has a unique crystal structure and exhibits novel physical properties, and is expected to be applied in thermoelectricity, magnetism, superconductivity and other fields. Attached Figure Description
[0036] Figure 1 The present invention is based on TiFe x Cu 2x-1 X-ray diffraction pattern of Sb-based thermoelectric materials;
[0037] Figure 2 The present invention is based on TiFe x Cu 2x-1 Electrical conductivity versus temperature curve of Sb-based thermoelectric materials;
[0038] Figure 3 The present invention is based on TiFe x Cu 2x-1 Seebeck coefficient curve of Sb-based thermoelectric materials as a function of temperature;
[0039] Figure 4 The present invention is based on TiFe x Cu 2x-1 Power factor curve of Sb-based thermoelectric material as a function of temperature;
[0040] Figure 5 The present invention is based on TiFe x Cu 2x-1 Thermal conductivity versus temperature curve of Sb-based thermoelectric materials;
[0041] Figure 6 The present invention is based on TiFe x Cu 2x-1 zT value of Sb-based thermoelectric material as a function of temperature;
[0042] Figure 7 The present invention is based on TiFe 0.7 Cu 0.4 Low-temperature resistivity and specific heat of Sb thermoelectric material as a function of temperature. Detailed Implementation
[0043] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. The following embodiments are implemented based on the technical solution of the present invention, providing detailed implementation methods and specific operating procedures; however, the scope of protection of the present invention is not limited to the following embodiments.
[0044] Example 1
[0045] In this embodiment, a P-type Hessler-like thermoelectric material with the chemical formula TiFe is described. 0.7 Cu 0.4 Sb.
[0046] In this embodiment, a p-type thermoelectric material TiFe 0.7 Cu 0.4 The method for preparing Sb involves high-energy ball milling (HEBM) and spark plasma sintering (SPS), and includes the following steps:
[0047] a. Calculation: Based on the stoichiometric ratio of Ti:Fe:Cu:Sb = 1:0.7:0.4:1 and the formula m = n × M, calculate 0.04 mol TiFe 0.7 Cu 0.4 The required mass of each element for Sb;
[0048] b. Sample preparation: In an argon glove box, weigh the Ti particles with a purity of 99.6%, Fe flakes with a purity of 99.99%, Cu particles with a purity of 99.99%, and Sb particles with a purity of 99.99% on an electronic balance with an accuracy of 0.1 mg according to the mass calculated in step a, and place the weighed raw materials into a stainless steel ball mill jar;
[0049] c. Alloying: The ball mill jar from step b is placed in a high-energy ball mill, and mixed powder is obtained by continuous and uninterrupted collision of balls and materials for 30 hours;
[0050] d. Sintering: The mixed powder obtained in step c is stored in an argon glove box. 1-1.5 grams of powder are weighed and placed in a graphite mold with a diameter of 12.7 mm. The mold is then placed in a spark plasma sintering (SPS) apparatus and a vacuum is applied. When the vacuum chamber pressure is approximately 60 MPa, pressure is slowly applied to the sample up to 6.3 kN to begin sintering. The sintering rate is 30-50 °C / min, reaching 700 °C in 20 minutes. After holding at this temperature for 10-15 minutes, the pressure is released, and the sample is allowed to cool naturally to room temperature, yielding TiFe with a diameter of 12.7 mm and a thickness of 1-2 mm. 0.7 Cu 0.4 Sb test disc.
[0051] Example 2
[0052] This embodiment is basically the same as the previous embodiments, except that:
[0053] In this embodiment, a P-type Hessler-like thermoelectric material with the chemical formula TiFe is described. 0.75 Cu 0.5 Sb.
[0054] In this embodiment, a p-type thermoelectric material TiFe 0.75 Cu 0.5 The method for preparing Sb involves high-energy ball milling (HEBM) and spark plasma sintering (SPS), and includes the following steps:
[0055] a. Calculation: Based on the stoichiometric ratio of Ti:Fe:Cu:Sb = 1:0.75:0.5:1 and the formula m = n × M, calculate 0.04 mol TiFe 0.75 Cu 0.5 The required mass of each element for Sb;
[0056] b. Sample preparation: This step is consistent with Example 1;
[0057] c. Alloying: This step is consistent with Example 1;
[0058] d. Sintering: The mixed powder obtained in step c is stored in an argon glove box. 1-1.5 grams of powder are weighed and placed in a graphite mold with a diameter of 12.7 mm. The mold is then placed in a spark plasma sintering (SPS) apparatus and a vacuum is applied. When the vacuum chamber pressure is approximately 60 MPa, pressure is slowly applied to the sample up to 6.3 kN to begin sintering. The sintering rate is 30-50 °C / min, reaching 700 °C in 20 minutes. After holding at this temperature for 10-15 minutes, the pressure is released, and the sample is allowed to cool naturally to room temperature, yielding TiFe with a diameter of 12.7 mm and a thickness of 1-2 mm. 0.75 Cu 0.5 Sb test disc.
[0059] Example 3
[0060] This embodiment is basically the same as the previous embodiments, except that:
[0061] In this embodiment, a P-type Hessler-like thermoelectric material with the chemical formula TiFe is described. 0.8 Cu 0.6 Sb.
[0062] In this embodiment, a p-type thermoelectric material TiFe 0.8 Cu 0.6 The method for preparing Sb involves high-energy ball milling (HEBM) and spark plasma sintering (SPS), and includes the following steps:
[0063] a. Calculation: Based on the stoichiometric ratio of Ti:Fe:Cu:Sb = 1:0.8:0.6:1 and the formula m = n × M, calculate 0.04 mol TiFe 0.8 Cu 0.6 The required mass of each element for Sb;
[0064] b. Sample preparation: This step is consistent with Example 1;
[0065] c. Alloying: This step is consistent with Example 1;
[0066] d. Sintering: The mixed powder obtained in step c is stored in an argon glove box. 1-1.5 grams of powder are weighed and placed in a graphite mold with a diameter of 12.7 mm. The mold is then placed in a spark plasma sintering (SPS) apparatus and a vacuum is applied. When the vacuum chamber pressure is approximately 60 MPa, pressure is slowly applied to the sample up to 6.3 kN to begin sintering. The sintering rate is 30-50 °C / min, reaching 700 °C in 20 minutes. After holding at this temperature for 10-15 minutes, the pressure is released, and the sample is allowed to cool naturally to room temperature, yielding TiFe with a diameter of 12.7 mm and a thickness of 1-2 mm. 0.8 Cu 0.6 Sb test disc.
[0067] Experimental test analysis:
[0068] The X-ray diffraction patterns tested in the above embodiments were all obtained on a Rigaku SmartLab-II diffractometer, and the X-ray source used was Cu-K. α Furthermore, the test samples were in powder form. The electrical performance tests in the above embodiments, including resistivity and Seebeck coefficient, were all performed on a ULVAC-RIKO ZEM-3 instrument. The electrical performance tests in the above embodiments, primarily testing the thermal diffusivity D, were all performed on a NETZSCH LFA467 instrument. The formula for calculating thermal conductivity is κ = DC. p ρ, where C p ρ represents the material's heat capacity, which can be estimated using the Dulong-Petty law, while ρ represents the material's density, which can be estimated using Archimedes' displacement method. The low-temperature resistivity and heat capacity measured in the above embodiments were performed using a Physical Property Measurement System (PPMS).
[0069] Figure 2-6 The above-described thermoelectric performance test results show that the conductivity of all test samples transitions from metallic to semiconductor conductivity between 600-700K. This is quite different from semiconductor thermoelectric materials. Consequently, the Seebeck coefficient of the test samples changes with temperature in the opposite direction to the conductivity, and all samples have a positive Seebeck coefficient, indicating that they are all P-type conductors dominated by holes.
[0070] The thermal conductivity of all tested samples decreased monotonically with temperature, indicating that bipolar diffusion was not observed. The trend is likely a result of various scattering methods, including phonon-phonon scattering, point defect scattering, and grain boundary scattering. Unlike conventional Hessler alloys where interstitial atoms are regularly half-filled or fully filled in interstitial positions, these Hessler-like alloys have interstitial atoms that fill interstitial positions randomly, resulting in some superior thermoelectric properties compared to conventional Hessler alloys. Analysis of the tested samples revealed that the overall thermal conductivity was not high. Compared to the intrinsic stoichiometric thermal conductivity of half-Hessler compounds (10-15 W / (m·K), the thermal conductivity of the samples tested in this invention ranged from 2.6-5.7 W / (m·K).
[0071] The test results show that the thermoelectric performance decreases with increasing Fe and Cu content in the interstitial spaces, particularly for TiFe. 0.7 Cu 0.4 Sb alloys exhibit the best performance: electrical conductivity between 46,000 and 65,000 S / m; Seebeck coefficient between 140 and 194 μV / K; and power factor between 11.6 and 20.8 μW / (cm·K). 2 The thermal conductivity is between 2.6 and 3.4 W / (m·K); the zT value is between 0.12 and 0.75. Thanks to the larger power factor and lower thermal conductivity at high temperatures, the zT value is also the highest at 973 K, reaching 0.75.
[0072] The present invention also measured the low-temperature physical properties of the component with the best performance. Figure 7 The graph shows the low-temperature physical properties of the sample prepared in Example 1 as a function of temperature. The resistivity and heat capacity in the graph change with temperature according to the following two rules:
[0073] i: The low-temperature resistivity of the tested component changes linearly with temperature;
[0074] ii: Low-temperature heat capacity C of the test component el / T changes logarithmically with temperature;
[0075] These two patterns are consistent with the temperature-dependent physical properties of non-Fermi liquid systems at low temperatures, further demonstrating that the alloy prepared in this invention possesses characteristics of non-Fermi liquid metals. This unusual metallic behavior generally exists in some special material systems and occurs near their quantum phase transition critical points. Conversely, it can be speculated that this invention may be able to find the quantum zero point of Fe / Cu system-like Hessler alloys through continuous compositional changes, and discover unusual physical properties such as superconductivity near the zero point.
[0076] In summary, this invention utilizes high-energy ball milling (HEBM) and spark plasma sintering (SPS) to efficiently synthesize TiFe. x Cu 2x-1 Sb (x = 0.7, 0.75, 0.8) is a pure phase with a Hessler-like structure, and these alloys exhibit high Seebeck coefficients, high electrical conductivity, and low thermal conductivity. One such alloy is composed of TiFe. 0.7 Cu 0.4 Sb alloys exhibit the highest thermoelectric properties, with a maximum power factor of 20.8 μW / (cm·K) at 973 K. 2 The lowest thermal conductivity is 2.6 W / (m·K), and the highest zT is 0.75. The random occupancy of Fe and Cu atoms in interstitial positions leads to a unique Hessler-like phase structure in this alloy. The presence of Fe, a magnetic atom, also imparts a degree of magnetism to the alloy. This results in the material studied in this invention possessing not only excellent thermoelectric properties but also unique physical properties. The heat capacity and resistivity tested at low temperatures show a linear relationship with temperature, indicating that the prepared thermoelectric material is not a semiconductor at low temperatures but rather an alloy with characteristics similar to a non-Fermi liquid metal. Therefore, the P-type TiFe studied in this invention... x Cu 2x-1 Sb alloys not only have great potential in the field of thermoelectrics, but also have the potential to be used in magnetic or superconducting applications due to their unique physical properties, making them a multifunctional material.
[0077] The embodiments of the present invention have been described above in conjunction with the accompanying drawings. However, the present invention is not limited to the above embodiments, and various changes can be made according to the purpose of the invention. Any changes, modifications, substitutions, combinations, or simplifications made based on the spirit and principle of the technical solution of the present invention should be considered equivalent substitutions, as long as they conform to the purpose of the invention and do not depart from the present invention's P-type TiFe x Cu 2x-1 The technical principles and inventive concepts of Sb-based thermoelectric materials and their preparation methods are all within the scope of protection of this invention.
Claims
1. A P-type Hessler-like thermoelectric material, characterized in that, Its chemical formula is: TiFe x Cu 2x-1 Sb, where x takes values in the range of 0.67 ≤ x ≤ 1.
2. The P-type Hessler-like thermoelectric material according to claim 1, characterized in that, In the chemical formulas mentioned, x = 0.7, 0.75, and 0.
8.
3. The P-type Hessler-like thermoelectric material according to claim 2, characterized in that, The electrical conductivity of the thermoelectric material is between 46,000 and 105,000 S / m, the Seebeck coefficient is between 10⁴ and 194 μV / K, and the power factor is between 10.3 and 20.8 μW / (cm·K). 2 The thermal conductivity is between 2.6 and 5.7 W / (m·K), and the zT value is between 0.07 and 0.
75.
4. The P-type Hessler-like thermoelectric material according to claim 2, characterized in that, In the chemical formula, x = 0.7, and the highest power factor at 973 K is 20.8 μW / (cm·K). 2 The lowest thermal conductivity is 2.6 W / (m·K), and the highest zT is 0.
75.
5. A method for preparing a P-type Hessler-like thermoelectric material as described in any one of claims 1 to 4, characterized in that, It is prepared using elemental Ti particles, Fe flakes, Cu particles, and Sb particles as raw materials by high-energy ball milling and spark plasma sintering.
6. The method for preparing the P-type Hessler-like thermoelectric material according to claim 5, characterized in that, Includes the following steps: a. Calculation: Based on the stoichiometric ratio of 1:x:(2x-1):1, calculate the mass of each element corresponding to a specific x value. b. Sample preparation: Weigh the elemental Ti particles, Fe flakes, Cu particles, and Sb particles according to the mass calculated in step a, and place the weighed raw materials in a stainless steel ball mill jar; c. Alloying: The ball mill jar from step b is placed in a high-energy ball mill and subjected to continuous ball milling and material collision for a long time to obtain mixed powder; d. Sintering: Weigh a certain amount of the mixed powder obtained in step c into a graphite mold, then place the mold into a spark plasma sintering device, evacuate it and apply a certain pressure to start sintering, and finally hold it at a certain temperature for a period of time, then release the pressure and let it cool naturally to room temperature to obtain the thermoelectric material.
7. The method for preparing the P-type Hessler-like thermoelectric material according to claim 6, characterized in that, In step b, the elemental Ti particles, Fe flakes, Cu particles, and Sb particles are weighed in an argon glove box according to the mass calculated in step a; the mixed powder obtained in step c is stored in an argon glove box.
8. The method for preparing the P-type Hessler-like thermoelectric material according to claim 6, characterized in that, In step d, the sintering gas pressure is 58-62 MPa and the applied pressure is 6-6.5 kN. The temperature is raised to 650-750℃ at a sintering rate of 30-50℃ / min and held for 10-15 min.
9. The method for preparing the P-type Hessler-like thermoelectric material according to claim 6, characterized in that, In step c, the ball milling time is set to 28-32 hours.
10. The method for preparing the P-type Hessler-like thermoelectric material according to claim 5, characterized in that, The purity of the elemental Ti particles, Fe flakes, Cu particles, and Sb particles are 99.6%, 99.99%, 99.99%, and 99.999%, respectively.
Citation Information
Patent Citations
High-entropy half-heusler thermoelectric material with low lattice thermal conductivity and preparation method thereof
AU2019101360A4
Method for connecting segmented thermoelectric materials
CN110098312A