Preparation and application of a reverse water gas shift catalyst with sodium and potassium as auxiliary agents

By adding sodium hydroxide or potassium hydroxide to a nickel, cobalt or platinum-based catalyst, and using titanium oxide, zirconium oxide or cerium oxide as a carrier, a catalyst with high CO selectivity and stability is prepared, solving the existing technical problems It solves the problem of poor CO selective control effect and achieves efficient CO2 conversion.

CN116351428BActive Publication Date: 2024-10-25DONGGUAN ZHENLIANG PRECISION TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310173190.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-27
Publication Date
2024-10-25
Estimated Expiration
2043-02-27

AI Technical Summary

Technical Problem

Existing nickel, cobalt or platinum-based catalysts have poor CO selectivity control effects in reverse water gas shift reactions, and the preparation of bimetallic catalysts is complex and not universal, resulting in low CO2 conversion rates.

Method used

Add sodium hydroxide or potassium hydroxide as an additive to a low-loading nickel, cobalt or platinum-based catalyst, combined with titanium oxide, zirconium oxide or cerium oxide as a carrier, and prepare the catalyst through specific synthesis steps to achieve high CO selectivity and stability.

Benefits of technology

It achieves high reactivity and nearly 100% CO selectivity in the reverse water gas shift reaction, and maintains good stability under high temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004099906430000011
    Figure HDA0004099906430000011
  • Figure HDA0004099906430000012
    Figure HDA0004099906430000012
  • Figure HDA0004099906430000021
    Figure HDA0004099906430000021
Patent Text Reader

Abstract

The present invention provides a supported catalyst A / MO for reverse water gas shift reaction 2 -X preparation method and application thereof, the catalyst composition comprises: active component A, auxiliary agent X and oxide carrier MO 2 , the active component A is nickel, cobalt or platinum, the auxiliary agent X is potassium or sodium, and the carrier MO 2 The catalyst A / M prepared by the present invention is cerium oxide, titanium oxide or zirconium oxide. 2 O x -X is used in the reverse water-gas shift reaction and exhibits excellent catalytic activity with a carbon monoxide (CO) selectivity close to 100%, which shows promising application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the preparation and application of a catalyst that can be used for reverse water-gas shift reaction, specifically, the synthesis of a catalyst A / MO2-X with nickel, cobalt or platinum as active component A, sodium or potassium as auxiliary agent X, titanium oxide, zirconium oxide or cerium oxide MO2 as carrier, and the application of the catalyst in high-selectivity reverse water-gas shift reaction. Background Art

[0002] As global fossil energy consumption continues to increase, CO2 emissions are also rising. As a typical greenhouse gas, its high concentration in the atmosphere will cause a series of environmental problems. However, from the perspective of resource utilization, CO2 is a large and cheap "carbon source". The catalytic conversion of CO2 is one of the most promising technical routes for reducing the concentration of CO2 in the atmosphere. CO is an excellent platform compound in C1 chemistry. With the help of the reverse water gas shift reaction (RWGS, CO2+H2→CO+H2OΔH 298K =41.3 kJ·mol -1 ) first reduces CO2 to more active CO, which can then be further hydrogenated into high-value-added chemicals such as olefins, aromatics, and gasoline. Therefore, the RWGS reaction is an important step in achieving carbon cycling.

[0003] At normal pressure, CO2 hydrogenation to produce CO and CH4 are competing reactions. The RWGS reaction can be regarded as an intermediate step in the methanation process because the generated CO can continue to be deeply hydrogenated into methane. Nickel-based catalysts and cobalt-based catalysts are typical methanation catalysts. Compared with copper-based catalysts commonly used in RWGS reactions, they are not easy to sinter under high temperature conditions and have attracted widespread attention from researchers (Journal of energy chemistry, 2016, 25 (4): 553-565; International journal of hydrogen energy, 2013, 38 (24): 10012-10018). In addition, the RWGS reaction is an endothermic reaction and often requires high temperature conditions. Although platinum-based catalysts have high CO selectivity under low temperature conditions, as the reaction temperature rises, the CO selectivity gradually decreases (Applied Catalysis B: Environmental, 2021, 291: 120101). The selective regulation of the above-mentioned nickel, cobalt or platinum catalysts for RWGS reactions at high temperatures has good application prospects.

[0004] It is generally believed that the CO2 hydrogenation reaction follows the CO intermediate mechanism, and the CO2 hydrogenation product depends on the adsorption strength of the CO intermediate: CO2 hydrogenation first generates the intermediate product CO, and the weakly adsorbed CO (*CO) is conducive to the rapid desorption of CO, thus showing a higher CO selectivity; while the stronger CO adsorption is conducive to further deep hydrogenation reduction to obtain CH4, showing a higher CH4 selectivity. Therefore, the essence of regulating the selectivity of CO2 hydrogenation products is to regulate the adsorption strength of the intermediate product *CO.

[0005] In order to promote the forward reaction of RWGS, researchers have proposed three selective control methods: reducing the size of metal particles (ACS Catal. 2013, 3, 2449-2455), using metal-support interaction (MSI) (Journal of Catalysis, 2019, 374: 60-71) and preparing bimetallic catalysts (CN109499577B, iScience, 2019, 17, 315-324). However, the disadvantages of the above control methods are that the CO2 conversion rate of the catalysts prepared by the first two methods is low (~10% at 500°C), and the preparation method of bimetallic catalysts is relatively complicated and not universal.

[0006] Studies have shown that adding sodium and potassium metal salts as additives to the catalyst is beneficial to the adsorption and activation of carbon dioxide, thereby improving the catalytic performance. Existing research has two conclusions: 1) The addition of sodium and potassium metal salts can promote the activity of the catalyst for the reverse water gas reaction and appropriately increase the selectivity of CO (<50%) (CN108144637A); 2) Sodium and potassium metal salts can promote methanation reactions by increasing the alkalinity of the carrier and introducing oxygen vacancies (CN101773833A; Catalysts, 2020, 10 (7): 812). However, in the current study, the addition of sodium and potassium metal salts can only improve the catalytic performance of the CO2 hydrogenation catalyst itself, and has not achieved nearly 100% CO selectivity regulation.

[0007] Based on the above research background, this work broke through the traditional selective regulation framework by adding sodium hydroxide or potassium hydroxide to low-loading nickel, cobalt or platinum-based catalysts, and synthesized a RWGS catalyst with high reactivity, high CO selectivity and good stability. Summary of the invention

[0008] The purpose of the present invention is to solve the existing technical problems and provide a preparation and application method of a catalyst A / MO2-X for reverse water-gas shift reaction. The catalyst has high reactivity in the reverse water-gas shift reaction, has a CO selectivity of nearly 100% and good stability.

[0009] In order to achieve the above-mentioned purpose of the present invention, the technical scheme adopted is as follows:

[0010] A method for synthesizing a catalyst A / MO2-X using nickel, cobalt or platinum as an active component A, sodium or potassium as an additive X, and titanium oxide, zirconium oxide or cerium oxide MO2 as a carrier, comprising the following steps:

[0011] 1. Synthesis of MO2:

[0012] 1) Take M precursor and ammonia water in deionized water, adjust pH to 8-11, and stir for 0.5-10h;

[0013] 2) Transfer the above solution into a centrifuge tube and wash with deionized water 1-10 times;

[0014] 3) drying the precipitate obtained above in an oven at 30°C-150°C;

[0015] 4) Calcine the dried solid at 400°C-900°C in air atmosphere for 1-10h to obtain a MO2 carrier.

[0016] 2. A method for preparing a catalyst, comprising the following steps:

[0017] 1) Take the active component precursor, auxiliary agent precursor and carrier MO2, dissolve them in deionized water, and stir them magnetically for 0.5-10h;

[0018] 2) drying the mixed solution in an oven at 30°C-150°C to obtain a solid catalyst precursor;

[0019] 3) The catalyst precursor is calcined in an air atmosphere at 400°C-900°C for 1-10 hours to obtain AO y / MO2-X(AO y is the oxide of A)

[0020] 4) The above AO y / MO2-X is placed in a hydrogen atmosphere at 400℃-900℃ for 1-5h to obtain A / MO2-X catalyst

[0021] 3. Application of catalyst

[0022] The catalyst obtained in step 4) is used for reverse water gas shift reaction. The evaluation conditions are as follows: after the catalyst is crushed into 40-80 meshes, 0.05-1g is taken and filled into a quartz tube, and placed in a fixed bed reactor for reaction evaluation. Carbon dioxide and hydrogen are used as reaction raw materials, the molar ratio of carbon dioxide: hydrogen = 1:4, and nitrogen is used as diluent gas; the gas hourly velocity GHSV is 1000-50000mL·h -1 ·g -1The reaction pressure is atmospheric pressure or near atmospheric pressure (0.1Mpa-1Mpa), and the reaction temperature is 300°C-800°C; the selectivity of carbon monoxide (CO) in the product obtained by the reaction is close to 100%. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 2 are XRD diagrams of Example 1 and Comparative Example 1 of the present invention.

[0024] Figure 2 This is the TEM image of Example 1 of the present invention.

[0025] Figure 3 The K element XPS graphs of Inventive Example 1 and Comparative Example 1.

[0026] Figure 4 It is a diagram of the catalytic performance of Example 1 of the present invention (right figure) and Comparative Example 1 (left figure).

[0027] Figure 5 The catalytic stability test diagrams of Example 1 (right figure) of the present invention and Comparative Example 1 (left figure) are shown.

[0028] Figure 6 The catalytic performance diagrams of Example 2 of the present invention (right figure) and Comparative Example 2 (left figure) are shown.

[0029] Figure 7 The catalytic performance diagrams of Example 3 (right figure) of the present invention and Comparative Example 3 (left figure) are shown. DETAILED DESCRIPTION

[0030] Embodiment 1:

[0031] 1) Synthesis of cerium oxide:

[0032] Weigh 2.5g of cerium nitrate in 100mL of deionized water, slowly add 2mL of ammonia water while stirring, and adjust the pH to 8. Continue stirring for 2h. Place the resulting mixed solution in a centrifuge tube and wash it three times by centrifugation at a speed of 9000r / min. Transfer the resulting precipitate to a watch glass, dry it at 60℃, place the resulting solid in a muffle furnace (air atmosphere), increase the temperature of the muffle furnace from room temperature to 500℃ at a heating rate of 5℃ / min and roast it for 2h to obtain a cerium oxide carrier.

[0033] 2) Preparation of catalyst Ni / CeO2-K:

[0034] Weigh 0.5g of cerium oxide, 0.0195g of nickel nitrate hexahydrate and 0.035g of potassium hydroxide, dissolve in 20mL of deionized water, and stir for 30 minutes to completely dissolve; place the above mixture in an oven at 60°C and dry for 12 hours to obtain a solid catalyst precursor; place the obtained catalyst precursor in a muffle furnace (air atmosphere), increase the temperature of the muffle furnace from room temperature to 500°C at a heating rate of 5°C / min and roast for 2 hours. The obtained sample is named NiO / CeO2-K. NiO / CeO2-K is reduced in a hydrogen atmosphere (a mixture of hydrogen and nitrogen, with a volume ratio of hydrogen in the mixture of 10%) at 500°C for 2 hours, and the final catalyst is named Ni / CeO2-K. Attached Figure 1 Figure 2 is the XRD pattern of Ni / CeO2-K catalyst, which shows that CeO2 was successfully synthesized, but no peak appeared due to the small Ni loading. Figure 2 TEM image of Ni / CeO2-K catalyst.

[0035] 3) Catalyst application:

[0036] The prepared Ni / CeO2-K was applied to the reverse water gas shift reaction. The catalyst was pressed and crushed into 40-80 mesh sizes, and 0.2 g was filled into a quartz tube reactor; the reaction gas was introduced at near atmospheric pressure (0.1 MPa), and the gas molar ratio was hydrogen: carbon dioxide: nitrogen = 4:1:5; the reaction temperature was 300℃-500℃, and the space velocity was 15000 mL·h -1 ·g -1 When the reaction temperature was 500°C, the CO2 conversion rate was 48.6% and the CO selectivity was 93.8%. After 20 hours of stability testing at 500°C, the CO2 conversion rate was 40.1% and the CO selectivity was 99.9%. Figure 4 The right figure is the catalytic performance diagram of Ni / CeO2-K (300℃-500℃; 15000mL·h -1 ·g -1 ). Figure 5 The right figure is the catalytic stability test diagram of Ni / CeO2-K (500℃; 15000mL·h -1 ·g -1 ).

[0037] Embodiment 2:

[0038] 1) Synthesis of cerium oxide, same as in Example 1

[0039] 2) Preparation of catalyst Pt / CeO2-K

[0040] Weigh 0.5g of cerium oxide, 0.0088g of platinum chloride and 0.035g of potassium hydroxide, dissolve in 20mL of deionized water, and stir for 30min to completely dissolve; place the above mixture in a 60°C oven and dry for 12h to obtain a solid catalyst precursor; place the obtained catalyst precursor in a muffle furnace (air atmosphere), increase the temperature of the muffle furnace from room temperature to 500°C at a heating rate of 5°C / min and roast for 2h, and the obtained sample is named PtO / CeO2-K. PtO / CeO2-K is reduced in a 500°C hydrogen atmosphere (a mixture of hydrogen and nitrogen, with a volume ratio of hydrogen in the mixture of 10%) for 2h, and the final catalyst is named Pt / CeO2-K.

[0041] 3) The catalyst application is the same as in Example 1. When the reaction temperature is 500°C, the CO2 conversion rate is 48.5% and the CO selectivity is 99.8%. Figure 6 The right figure shows the catalytic performance of Pt / CeO2-K (300℃-500℃; 15000mL·h -1 ·g -1 ).

[0042] Embodiment 3:

[0043] 1) Synthesis of titanium oxide:

[0044] Weigh 1.09g of titanium tetrachloride in 100mL of deionized water, slowly add 2mL of ammonia water while stirring, and adjust the pH to 8. Continue stirring for 2h. Place the resulting mixed solution in a centrifuge tube and wash it three times by centrifugation at a speed of 9000r / min. Transfer the resulting precipitate to a watch glass, dry it at 60℃, place the resulting solid in a muffle furnace (air atmosphere), increase the temperature of the muffle furnace from room temperature to 500℃ at a heating rate of 5℃ / min and roast it for 2h to obtain a titanium oxide carrier.

[0045] 2) Preparation of catalyst Ni / TiO2-Na:

[0046] Weigh 0.5g titanium oxide, 0.0195g nickel nitrate hexahydrate and 0.025g sodium hydroxide, dissolve in 20mL deionized water, stir for 30min to completely dissolve; place the above mixture in a 60°C oven and dry for 12h to obtain a solid catalyst precursor; place the obtained catalyst precursor in a muffle furnace (air atmosphere), increase the temperature of the muffle furnace from room temperature to 500°C at a heating rate of 5°C / min and roast for 2h, and the obtained sample is named NiO / TiO2-Na. NiO / TiO2-Na is reduced in a 500°C hydrogen atmosphere (a mixture of hydrogen and nitrogen, with a volume ratio of hydrogen in the mixture of 10%) for 2h, and the final catalyst is named Ni / TiO2-Na.

[0047] 3) The catalyst application is the same as in Example 1. When the reaction temperature is 500°C, the CO2 conversion rate is 36.2% and the CO selectivity is 95.7%. Figure 7 The right figure is the catalytic performance diagram of Ni / TiO2-Na (300℃-500℃; 15000mL·h -1 ·g -1 ).

[0048] Comparative Example 1:

[0049] As a comparative experimental group, a synthesis method similar to that of the above-mentioned Example 1 was adopted, except that potassium hydroxide was not added.

[0050] 1) Synthesis of cerium oxide, same as in Example 1

[0051] 2) Preparation of Ni / CeO2 catalyst

[0052] Weigh 0.5g of cerium oxide and 0.0195g of nickel nitrate hexahydrate, dissolve in 20mL of deionized water, and stir for 30min to completely dissolve; place the above mixture in a 60°C oven and dry for 12h to obtain a solid catalyst precursor; place the obtained catalyst precursor in a muffle furnace (air atmosphere), increase the temperature of the muffle furnace from room temperature to 500°C at a heating rate of 5°C / min and roast for 2h, and the obtained sample is named NiO / CeO2. NiO / CeO2 is reduced in a 500°C hydrogen atmosphere (a mixture of hydrogen and nitrogen, with a volume ratio of hydrogen in the mixture of 10%) for 2h, and the final catalyst is named Ni / CeO2.

[0053] 3) Catalyst application, the same as in Example 1. When the reaction temperature is 500°C, the CO2 conversion rate is 55.0% and the CO selectivity is 24.5%. After 20 hours of stability testing at 500°C, the CO2 conversion rate is 49.8% and the CO selectivity is 18.7%. Figure 4 The left figure is the catalytic performance diagram of Ni / CeO2 (300℃-500℃; 15000mL·h -1 ·g -1 ). Figure 5 The left figure is the catalytic stability test diagram of Ni / CeO2 (500℃; 15000mL·h -1 ·g -1 ).

[0054] Comparative Example 2:

[0055] As a comparative experimental group, a synthesis method similar to that of the above-mentioned Example 2 was adopted, except that potassium hydroxide was not added.

[0056] 1) Synthesis of cerium oxide, same as in Example 1

[0057] 2) Preparation of Pt / CeO2 catalyst

[0058] Weigh 0.5g of cerium oxide and 0.0088g of platinum chloride, dissolve in 20mL of deionized water, and stir for 30min to completely dissolve; place the above mixture in a 60°C oven and dry for 12h to obtain a solid catalyst precursor; place the obtained catalyst precursor in a muffle furnace (air atmosphere), increase the temperature of the muffle furnace from room temperature to 500°C at a heating rate of 5°C / min and roast for 2h, and the obtained sample is named PtO2 / CeO2. PtO2 / CeO2 is placed in a 500°C hydrogen atmosphere (a mixture of hydrogen and nitrogen, with a volume ratio of hydrogen in the mixture of 10%) for reduction for 2h, and the final catalyst is named Pt / CeO2.

[0059] 3) The catalyst application is the same as in Example 1. When the reaction temperature is 500°C, the CO2 conversion rate is 49.3% and the CO selectivity is 50.2%. Figure 6 The left figure shows the catalytic performance of Pt / CeO2 (300℃-500℃; 15000mL·h -1 ·g -1 ).

[0060] Comparative Example 3:

[0061] As a comparative experimental group, a synthesis method similar to that of the above-mentioned Example 3 was adopted, except that no sodium hydroxide was added.

[0062] 1) Synthesis of titanium oxide, same as in Example 3

[0063] 2) Preparation of catalyst Ni / TiO2:

[0064] Weigh 0.5g titanium oxide and 0.0195g nickel nitrate hexahydrate, dissolve in 20mL deionized water, and stir for 30min to completely dissolve; place the mixture in a 60°C oven and dry for 12h to obtain a solid catalyst precursor; place the obtained catalyst precursor in a muffle furnace (air atmosphere), increase the temperature of the muffle furnace from room temperature to 500°C at a heating rate of 5°C / min and roast for 2h, and the obtained sample is named NiO / TiO2. NiO / TiO2 is reduced in a 500°C hydrogen atmosphere (a mixture of hydrogen and nitrogen, with a volume ratio of hydrogen in the mixture of 10%) for 2h, and the final catalyst is named Ni / TiO2.

[0065] 3) The catalyst application is the same as in Example 1. When the reaction temperature is 500°C, the CO2 conversion rate is 20.7% and the CO selectivity is 48.8%. Figure 7The left figure is the catalytic performance diagram of Ni / TiO2 (300℃-500℃; 15000mL·h -1 ·g -1 ).

[0066] Obviously, the above experimental examples are only examples for clear explanation, and are not intended to limit the implementation methods. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from this are still within the protection scope of the invention.

Claims

1. A method for improving the catalytic stability of a reverse water gas shift reaction, comprising the following steps: 1) Synthesis of cerium oxide: Weigh 2.5 g of cerium nitrate in 100 mL of deionized water, slowly add 2 mL of ammonia water while stirring, adjust the pH to 8, continue stirring for 2 h, place the resulting mixed solution in a centrifuge tube, wash it three times by centrifugation at a speed of 9000 r / min, transfer the resulting precipitate to a watch glass, dry it at 60 ° C, place the resulting solid in a muffle furnace, increase the temperature of the muffle furnace from room temperature to 500 ° C at a heating rate of 5 ° C / min and calcine it for 2 h to obtain a cerium oxide carrier; 2) Preparation of catalyst Ni / CeO2-K: Weigh 0.5g of cerium oxide, 0.0195g of nickel nitrate hexahydrate and 0.035g of potassium hydroxide, dissolve in 20mL of deionized water, and stir for 30min to completely dissolve; place the above mixture in an oven at 60°C and dry for 12h to obtain a solid catalyst precursor; place the obtained catalyst precursor in a muffle furnace, increase the temperature of the muffle furnace from room temperature to 500°C at a heating rate of 5°C / min and calcine for 2h to obtain NiO / CeO2-K; place NiO / CeO2-K in a hydrogen atmosphere at 500°C for 2h to obtain the final catalyst Ni / CeO2-K; 3) Catalytic stability test: The prepared Ni / CeO2-K was applied to the reverse water gas shift reaction; the catalyst was tableted and crushed into 40-80 mesh sizes, and 0.2 g was filled into a quartz tube reactor; the reaction gas was introduced at near normal pressure, and the gas molar ratio of the reaction gas was hydrogen: carbon dioxide: nitrogen = 4:1:5; the reaction temperature was 300°C-500°C, and the space velocity was 15000 mL·h -1 ·g -1 ; When the reaction temperature was 500°C, the CO2 conversion rate was 48.6% and the CO selectivity was 93.8%; after 20 hours of stability testing at 500°C, the CO2 conversion rate was 40.1% and the CO selectivity was 99.9%.