A high-flexural geopolymer-based organic-inorganic composite plate and preparation method thereof

By using the pressure-vibration-vacuum pumping three-dimensional field coupling process in geopolymers and the vibration and compression molding of organic-inorganic composite plastic slurries, the problems of low flexural strength and high brittleness of geopolymers are solved, and the resistance is significantly improved. Flexural strength and toughness achieve efficient toughening effect of inorganic cementitious materials.

CN116354694BActive Publication Date: 2024-10-11SOUTH CHINA UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310309465.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-11
Estimated Expiration
2043-03-28

AI Technical Summary

Technical Problem

The application of geopolymers in modern construction projects is limited by their low flexural strength and high brittleness, and existing technologies have limited effects in improving flexural strength and toughness.

Method used

The experimental small press process of pressure-vibration-vacuum water pumping three-dimensional field coupling operation is combined with the mixing of slag, water glass and retarder, adding organic solutions containing active groups, and forming through vibration and compression of organic-inorganic composite plastic slurry. , prepare organic-inorganic composite gelling sheets without macroscopic defects, and improve the strength and toughness of inorganic gelling materials.

Benefits of technology

It significantly improves the flexural strength and toughness of geopolymer-based organic-inorganic composite sheets, unifies and balances the high flexural strength and high toughness of inorganic cementitious materials, and extends the service life and scope of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116354694B_ABST
    Figure CN116354694B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of building materials, and discloses a high-flexural geopolymer-based organic-inorganic composite board and a preparation method thereof. The present invention adds organic matter containing active groups to the slurry, and utilizes the pressure-vibration-vacuum pumping three-dimensional field coupling of a small experimental press to enhance the organic-inorganic chemical reaction, thereby preparing an organic-inorganic composite board that achieves unity and balance in terms of high flexural strength and high toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and particularly relates to a high-flexural-resistance geopolymer-based organic-inorganic composite plate and a preparation method thereof. Background Art

[0002] Geopolymer is a kind of clinker-free cement, which is low-carbon, environmentally friendly and high-performance. Its development and utilization is in line with the direction of social development. It also has excellent early compressive strength, low permeability, corrosion resistance, high temperature resistance and other properties. However, geopolymer has problems such as low flexural strength and high brittleness, which limits its application in modern construction projects instead of cement.

[0003] In recent years, organic matter has been added to inorganic gelling materials to form films and bond them, and evenly distributed in the inorganic gelling material matrix, which improves the energy consumption capacity of the inorganic gelling material matrix for crack expansion, thereby playing a toughening role. In addition, organic matter can react chemically with the hydration products of inorganic gelling materials, fill microcracks or defects, and form an organic-inorganic interpenetrating cross-linked network structure, which improves the flexural strength of geopolymers and opens up new directions for the toughening research of geopolymers.

[0004] Combined with the current research status, it can be seen that even if organic matter is added to inorganic gelling materials to prepare organic-inorganic composite gelling materials using ordinary molding processes, the flexural strength can be improved, but it is very limited, and the increase in flexural strength is only about 25%. In addition, there is no obvious improvement and research on toughness. Summary of the invention

[0005] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a method for preparing a high-flexural-resistance geopolymer-based organic-inorganic composite board.

[0006] Another object of the present invention is to provide a high-flexural-resistance geopolymer-based organic-inorganic composite board prepared by the above method.

[0007] The purpose of the present invention is achieved through the following solutions:

[0008] A method for preparing a high-flexural geopolymer-based organic-inorganic composite plate comprises the following steps:

[0009] (1) Mix slag, water glass, retarder and water, and stir until the mixture is uniform to obtain slurry;

[0010] (2) mixing the slurry prepared in (1) and an organic solution containing active groups, and stirring to obtain an organic-inorganic composite plastic slurry;

[0011] (3) pouring the organic-inorganic composite plastic slurry into a fixed iron mold of a small experimental press to vibrate, evacuate and press to obtain a plate of fixed size;

[0012] (4) Covering the surface of the plate obtained in step (3) with a waterproof film and curing it to obtain a high-flexural-resistance geopolymer-based organic-inorganic composite plate.

[0013] The water glass modulus in step (1) is 1.0-2.0.

[0014] The amount of water glass used in step (1) is 2%-10% of the mass of the slag.

[0015] The retarder in step (1) includes at least one of barium chloride, sodium hexametaphosphate and lignin sulfonate.

[0016] The amount of the retarder in step (1) is 0.5%-2% of the mass of the slag.

[0017] The stirring time in step (1) is 2-10 min, preferably 2 min.

[0018] The organic matter containing active groups in step (2) includes one or two of sodium polyacrylate (PAA-Na) and silane coupling agent; wherein the silane coupling agent includes at least one of KH550, KH560, and KH570.

[0019] The amount of organic matter containing active groups in step (2) is 2%-20% of the mass of the slag.

[0020] The total amount of water used in step (1) and step (2) satisfies: the mass ratio of water to slag in the organic-inorganic composite plastic slurry in step (2) is 0.1-0.5.

[0021] The stirring time in step (2) is 2-10 min, preferably 3 min.

[0022] After the stirring in step (2), the mixture is allowed to stand for 5-60 minutes until a plastic slurry with hard plastic properties (0 < liquid plastic index < 0.25) is formed.

[0023] The frequency of the experimental small press in step (3) is set to 5Hz-50Hz, the vibration time is 2min-30min, and the pressure is 0.1MPa-1MPa.

[0024] The curing in step (4) is first steam curing for 12-24 hours and then curing at room temperature for 6-30 days; wherein the steam curing temperature is 40-80°C.

[0025] The high-flexural-resistance geopolymer-based organic-inorganic composite board prepared by the above method.

[0026] Mechanism of the present invention:

[0027] By using the experimental small press with the coupling effect of pressure-vibration-vacuum pumping three-dimensional field, the water content is reduced, the pores are eliminated, the organic-inorganic chemical reaction is enhanced, and the organic-inorganic composite cementitious sheet without macroscopic defects is prepared. This greatly improves the strength and toughness of inorganic cementitious materials, and prolongs and increases the service life and range of inorganic cementitious materials.

[0028] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0029] The high flexural geopolymer-based organic-inorganic composite plate of the present invention has high flexural strength and can also improve the toughness of inorganic gelling materials, so that the inorganic gelling materials can achieve unity and balance in terms of high flexural strength and high toughness. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] FIG. 1( a ) is a bar graph showing the flexural strength performance of the slag-based organic-inorganic composite panels prepared in Comparative Examples 1 and 2.

[0031] FIG1( b ) is a bar graph showing the flexural strength performance of the slag-based organic-inorganic composite plates prepared in Comparative Example 2 and Examples 1-4.

[0032] FIG1( c ) is a bar graph showing the flexural strength performance of the slag-based organic-inorganic composite plates prepared in Comparative Example 2 and Examples 5-7.

[0033] FIG. 2( a ) is a bending load-bending displacement curve diagram of the organic-inorganic composite plate materials prepared in Comparative Example 2 and Examples 1-4.

[0034] FIG. 2( b ) is a bending load-bending displacement curve diagram of the organic-inorganic composite plates prepared in Comparative Example 2 and Examples 5-7.

[0035] FIG. 3( a ) is a graph showing the fracture toughness of the organic-inorganic composite plates prepared in Comparative Example 2 and Examples 1-7.

[0036] FIG3( b ) is a fracture energy diagram of the organic-inorganic composite plates prepared in Comparative Example 2 and Examples 1-7.

[0037] Figure 4 Schematic diagram of the main reaction steps. DETAILED DESCRIPTION

[0038] The present invention is further described in detail below in conjunction with the examples and drawings, but the embodiments of the present invention are not limited thereto. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0039] Unless otherwise specified, the reagents used in the examples can be purchased from the market.

[0040] The experimental small press used in the present invention was purchased from Foshan Huigu Co., Ltd.

[0041] The water glass solution with a modulus of 3.34 was purchased from Foshan Zhongfa Water Glass Factory. The original modulus was 3.34, the Na2O content was 8.94%, the SiO2 content was 28.93%, and the solid content was 37.86%.

[0042] PAA-Na: purchased from Shanghai McLean, mass concentration is 50%, 3000Mw.

[0043] KH550: purchased from Shanghai McLean, mass concentration 97%; KH560: purchased from Shanghai McLean, mass concentration 97%; KH570: purchased from Shanghai McLean, mass concentration 97%.

[0044] Comparative Example 1

[0045] The specific steps of preparing a slag-based inorganic plate include:

[0046] (1) Dissolve 161.6 g of sodium hydroxide in 1285.2 g of the original 3.34 modulus water glass solution to prepare a 1.6 modulus water glass solution, and weigh 6% of the slag mass of 1.6 modulus water glass, and let it stand for 24 hours for use;

[0047] (2) Weigh 1% of the mass of slag and dissolve it in water, and let it stand for use;

[0048] (3) 4000 g of slag and the solution obtained in step (1) and step (2) were fully stirred in a stirrer for 5 min to obtain a uniformly mixed slurry, wherein the total water content of the obtained slurry was 1000 g, and the mass ratio of water to slag was 0.25;

[0049] (4) Place the slurry in step (3) in a 300mm*300mm*25mm mold and let it stand for 6 minutes. Steam cure at 60°C for 1 day, and then cure at room temperature for 7 days and 28 days to obtain a slag-based inorganic sheet.

[0050] Comparative Example 2

[0051] The specific steps of preparing a slag-based inorganic plate include:

[0052] (1) Dissolve 161.6 g of sodium hydroxide in the original 3.2 modulus water glass solution to prepare a 1.6 modulus water glass solution, and weigh 6% of the slag mass of 1.6 modulus water glass, and let it stand for 24 hours for use;

[0053] (2) Weigh 1% of the mass of slag in barium chloride and dissolve it in water, then let it stand for later use;

[0054] (3) 4000 g of slag and the solution obtained in step (1) and step (2) were fully stirred in a mixer for 5 min to obtain a uniformly mixed slurry;

[0055] (4) The slurry in step (3) is allowed to stand for 6 minutes to obtain a plastic slurry with hard plastic properties (0 < liquid plasticity index < 0.25), the total water content of the obtained plastic slurry is 1000 g, and the mass ratio of water to slag is 0.25; the plastic slurry is placed in a 300mm*300mm*25mm mold, and placed in a small experimental press. The parameters of the small experimental press are set to 18 Hz, the vibration time is 5 minutes, and the pressure is 1 MPa.

[0056] (5) Steam curing at 60°C for 1 day, and then curing at room temperature for 7 days and 28 days to obtain slag-based inorganic plates.

[0057] Example 1

[0058] The specific steps of preparing a slag-based organic-inorganic composite gelling material include:

[0059] (1) Dissolve 161.6 g of sodium hydroxide in the original 3.2 modulus water glass solution to prepare a 1.6 modulus water glass solution, and weigh 6% of the slag mass of 1.6 modulus water glass, and let it stand for 24 hours for use;

[0060] (2) Weigh 1% of the mass of slag in barium chloride and dissolve it in water, then let it stand for later use;

[0061] (3) 4000 g of slag and the solution obtained in step (1) and step (2) were fully stirred in a mixer for 2 min to obtain a uniformly mixed slurry;

[0062] (4) Weigh 7% of the slag mass of PAA-Na (7% of PAA-Na is the actual amount of PAA-Na not including water) and dissolve it in water, and let it stand for use;

[0063] (5) adding the PAA-Na solution obtained in step (4) to the mixed slurry of step (3), continuing to stir fully for 3 minutes, and standing for 16 minutes to obtain an organic-inorganic composite plastic slurry with hard plastic properties (0 < liquid plastic index < 0.25), wherein the total water content of the obtained plastic slurry is 1000 g, and the mass ratio of water to slag is 0.25;

[0064] (6) The slurry in step (5) was placed in a mold of 300 mm × 300 mm × 25 mm and placed in a small experimental press. The parameters of the small experimental press were set to 18 Hz, the vibration time was 5 min, and the pressure was 1 MPa.

[0065] (7) The board obtained in step (6) was steam-cured at 60° C. for 1 day, and then cured at room temperature for 7 days and 28 days.

[0066] Example 2

[0067] The preparation process of this embodiment is basically the same as that of embodiment 1, except that the organic matter in step (4) is KH550.

[0068] Example 3

[0069] The preparation process of this embodiment is basically the same as that of embodiment 1, except that the organic matter in step (3) is KH560.

[0070] Example 4

[0071] The preparation process of this embodiment is basically the same as that of embodiment 1, except that the organic matter in step (3) is KH570.

[0072] Example 5

[0073] The preparation process of this embodiment is basically the same as that of embodiment 1, except that the organic matter in step (3) is 5% KH550+2% PAA-Na.

[0074] Example 6

[0075] The preparation process of this embodiment is basically the same as that of embodiment 1, except that the organic matter in step (3) is 5% KH560+2% PAA-Na.

[0076] Example 7

[0077] The preparation process of this embodiment is basically the same as that of embodiment 1, except that the organic matter in step (3) is 5% KH570+2% PAA-Na.

[0078] Comparing the flexural strength of Comparative Example 1 and Comparative Example 2 using the common molding process and the pressure-vibration-vacuum pumping three-dimensional coupling process, see Figure 1 (a), the 7d and 28d flexural strengths of Comparative Example 1 and Comparative Example 2 are 3.12MPa, 4.21MPa and 3.24MPa, 5.39MPa respectively. The pressure-vibration-vacuum pumping three-dimensional coupling process can improve the flexural strength.

[0079] Comparing the flexural strength of the pressure-vibration-vacuum pumping three-dimensional field coupling molding process of comparative example 2 and the embodiment, see Figure 1 (b) and Figure 1 (c), the 7d and 28d flexural strengths of comparative example 2 are 4.21MPa and 5.39MPa respectively, the 7d flexural strengths of embodiments 1-4 are 6.38MPa, 6.81MPa, 4.82MPa and 8.56MPa respectively, and the 28d flexural strengths are 7.64MPa, 10.38MPa, 7.85MPa and 10.89MPa respectively. The 7d flexural strengths of embodiments 5-7 are 17.78MPa, 10.41MPa and 16.12MPa respectively, and the 28d flexural strengths are 19.68MPa, 12.51MPa and 21.35MPa respectively. It shows that the addition of two-component organic matter can greatly improve the flexural strength of slag-based geopolymers by using the vibration vacuum pressing molding process.

[0080] The bending load-bending displacement curves of Comparative Example 2 and Examples 1-4 are shown in FIG2(a). Compared with the comparative example, the addition of KH550 (Example 2) and KH570 (Example 4) increases the bending displacement from 0.032 mm to 0.035 mm and 0.056 mm, respectively, under a load of 19.14 N, by 9.36% and 75%, respectively. The maximum bending loads of PAA-Na (Example 1) and KH560 (Example 3) are 7.72 N and 5.60 N, respectively, which are less than the load in Comparative Example 2. This is because the addition of PAA-Na and KH560 reduces the strength of the sheet. However, compared with Comparative Example 2, under a load of 5.56 N, the bending displacements are 0.012 mm, 0.040 mm and 0.057 mm, respectively, which is significantly increased. The addition of a single-component organic matter significantly increases the toughness of the inorganic gelling material.

[0081] The bending load-bending displacement curves of Comparative Example 2 and Examples 5-7 are shown in Figure 2 (b). Compared with Comparative Example 2, Example 1, Example 4 and Example 6, the addition of KH570+PAA-Na (Example 7) increases the maximum bending load to 25.78N, which is 32.61%, 233%, 19.13% and 6.98% higher than Comparative Example 2, Example 1, Example 4 and Example 6, respectively. The corresponding bending displacement increases to 0.083mm, which is 166%, 50.91%, 34.92% and 21.43% higher than Comparative Example 2, Example 1, Example 4 and Example 6, respectively. The essential reason why the toughness of Example 7 is better than that of Examples 5 and 6 is that KH570 contains acryloxy groups that can combine with the organic PAA-Na. In addition, under alkaline conditions, the highly active silanol produced by hydrolysis can react chemically with the CASH gel, a slag reaction product, to act as a silane coupling agent and form an organic-inorganic composite network structure.

[0082] According to the fracture toughness and fracture energy bar graphs of Comparative Example 2 and Examples 1-7, Figure 3(a) and Figure 3(b) show that the fracture toughness and fracture energy of Example 7 are 0.665 MPa*m 1 / 2 and 102.77N / m. From the perspective of toughening, it can be seen that the organic-inorganic composite board prepared by the two-component organic KH570+PAA-Na composite slag-based inorganic cementitious material using the pressure-vibration-vacuum pumping three-dimensional field coupling experimental small press has the characteristics of high flexural resistance and high toughness.

[0083] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a geopolymer-based organic-inorganic composite plate, characterized in that The following steps are involved: (1) Mix slag, water glass, retarder and water, and stir until the mixture is uniform to obtain slurry; (2) mixing the slurry prepared in (1) and an organic solution containing active groups, and stirring to obtain an organic-inorganic composite plastic slurry; (3) pouring the organic-inorganic composite plastic slurry into a fixed iron mold of a small experimental press for vibration, vacuuming and pressing to obtain a plate of fixed size; (4) Covering the surface of the plate obtained in step (3) with a waterproof film and curing it to obtain a high-flexural-resistance geopolymer-based organic-inorganic composite plate; The organic matter containing active groups in step (2) is sodium polyacrylate and a silane coupling agent; The amount of water glass used in step (1) is 2%-10% of the mass of the slag; The amount of the retarder in step (1) is 0.5%-2% of the mass of the slag; The amount of the organic matter containing active groups in step (2) is 2%-20% of the mass of the slag; The silane coupling agent includes at least one of KH550, KH560 and KH570.

2. The preparation method according to claim 1, characterized in that: The water glass modulus in step (1) is 1.0-2.

0.

3. The preparation method according to claim 1, characterized in that: The retarder in step (1) includes at least one of barium chloride, sodium hexametaphosphate, and lignin sulfonate.

4. The preparation method according to claim 1, characterized in that: The total amount of water used in step (1) and step (2) satisfies: the mass ratio of water to slag in the organic-inorganic composite plastic slurry in step (2) is 0.1-0.

5.

5. The preparation method according to claim 1, characterized in that: After the stirring in step (2), the mixture is allowed to stand for 5-60 minutes until a plastic slurry with hard plastic properties is formed.

6. The preparation method according to claim 1, characterized in that: The frequency of the experimental small press in step (3) is set to 5 Hz-50 Hz, the vibration time is 2 min-30 min, and the pressure is 0.1 MPa-1 MPa.

7. The preparation method according to claim 1, characterized in that: The curing in step (4) is first steam curing for 12-24 hours and then curing at room temperature for 6-30 days; wherein the steam curing temperature is 40-80°C.

8. A geopolymer-based organic-inorganic composite board prepared according to the method according to any one of claims 1 to 7.