A low-mold-scale halogen-free flame-retardant reinforced nylon material and preparation method thereof

By introducing isomers of zirconium hydroxide into halogen-free flame retardant reinforced nylon materials, the mold scale problem caused by the decomposition reaction of the material during processing is solved, the stability and flame retardant performance of the product are maintained, and the production is improved Efficiency, suitable for the manufacturing of electronic and electrical parts.

CN116355405BActive Publication Date: 2024-11-26KINGFA SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310412747.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2024-11-26
Estimated Expiration
2043-04-18

AI Technical Summary

Technical Problem

Halogen-free flame retardant reinforced nylon materials are prone to decomposition reactions during processing, producing acidic substances and small molecular substances, resulting in accumulation of mold scales, reducing product purity and production efficiency, and the polarity difference of modified halogen-free flame retardant components affects the product uniformity and mechanical properties.

Method used

Introduced special compositions of inorganic zirconium hydroxide, including α-[Zr(OH)4], β-[Zr4O2(OH)12] and γ-[Zr4O4(OH)8], these isomers are fixed by adsorption reactions Acid substances and small molecule substances avoid degradation of nylon resin and add them to nylon resin, glass fiber and halogen-free flame retardant at appropriate amounts to maintain the stability and flame retardant properties of the product.

Benefits of technology

It significantly reduces the amount of mold scale generated during the injection molding process, improves production efficiency, and improves the stability and flowability of the material without affecting the tensile strength and flame retardant properties of the product. It is suitable for electronic and electrical parts. manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004183783940000061
    Figure BDA0004183783940000061
  • Figure BDA0004183783940000062
    Figure BDA0004183783940000062
  • Figure BDA0004183783940000071
    Figure BDA0004183783940000071
Patent Text Reader

Abstract

The invention discloses a low mold scale halogen-free flame retardant reinforced nylon material and a preparation method thereof, belonging to the technical field of polymer materials. The material introduces a special composition of inorganic zirconium hydroxide without changing the halogen-free flame retardant component or processing technology. The component can fix acidic substances and decomposed small molecular substances, and then reacts with the acidic substances generated by the decomposition of the halogen-free flame retardant component through the three special components it contains, ultimately avoiding the degradation of nylon resin in the product, reducing the amount of mold scale generated during the production injection molding process, and not affecting the tensile strength and flame retardant properties of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a low-mold-scale halogen-free flame-retardant reinforced nylon material and a preparation method thereof. Background Art

[0002] Halogen-free flame-retardant reinforced nylon materials generally refer to nylon materials with high flame retardancy, high strength and environmental friendliness, which are prepared by using halogen-free flame-retardant ingredients as raw materials and combining them with reinforcing fillers (such as glass fiber, talcum powder, etc.). However, since the halogen-free flame-retardant ingredients in the material are prone to decomposition reactions and produce acidic substances during processing, the nylon resin as the main component is degraded and its performance is reduced. At the same time, the small molecular substances produced by the decomposition will continue to accumulate in the production injection mold to produce mold scale, which reduces the purity of the product and even requires frequent mold cleaning, significantly reducing production efficiency.

[0003] In order to solve the above problems, people have tried to reduce the decomposition reaction of halogen-free flame retardant components and the formation of mold deposit by modifying the chemical properties of halogen-free flame retardant components or introducing alkaline neutralizers with high compatibility with nylon resins. However, due to the high processing temperature of halogen-free flame retardant reinforced nylon materials themselves, the effect of modification is limited. At the same time, the polarity of the modified halogen-free flame retardant components is easily different from the polarity of the reinforcing filler, resulting in lower uniformity of the components of the final product, and even affecting the mechanical properties (especially tensile strength) and flame retardant properties of the product. In addition, some people have tried to reduce the generation of mold deposit by step-by-step melting based on the original formula, but such a process is time-consuming and requires multiple heating intervals, which consumes too much energy. Summary of the invention

[0004] Based on the defects of the prior art, the purpose of the present invention is to provide a low mold deposit halogen-free flame retardant reinforced nylon material. Without changing the halogen-free flame retardant component or processing technology, the material introduces an inorganic zirconium hydroxide of a special composition, which can fix acidic substances and decomposed small molecular substances, and then reacts with the acidic substances produced by the decomposition of the halogen-free flame retardant component through the three special components it contains, thereby ultimately avoiding the degradation of the nylon resin in the product and reducing the amount of mold deposit generated during the production injection molding process. At the same time, it will not affect the intrinsic tensile strength and flame retardant properties of the product.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] A low-mold-deposit halogen-free flame-retardant reinforced nylon material, comprising the following components in parts by weight:

[0007] 40-60 parts of nylon resin, 20-40 parts of glass fiber, 14-20 parts of halogen-free flame retardant, 0.1-1 parts of zirconium hydroxide and 0.8-2 parts of processing aid; the zirconium hydroxide is a mixture of isomers, including α-[Zr(OH)4], β-[Zr4O2(OH) 12 ]andγ-[Zr4O4(OH)8].

[0008] Zirconium hydroxide is a water-insoluble and amphoteric hydroxide that can react with acidic substances. However, it has three isomers, namely α-[Zr(OH)4], β-[Zr4O2(OH) 12 ] and γ-[Zr4O4(OH)8]. The chemical activities of the three are different due to their crystal structure. Generally, α-[Zr(OH)4], β-[Zr4O2(OH) 12 ] and γ-[Zr4O4(OH)8] decrease in activity in turn. Theoretically, the most active α-[Zr(OH)4] should have the best effect. However, in the components of the low-scale halogen-free flame-retardant reinforced nylon material of the present invention, since the thermal decomposition of the halogen-free flame retardant is not instantaneous, both the acidic substances produced and the small molecular substances obtained after decomposition are continuously increased, and zirconium hydroxide needs to continue to act at an appropriate adsorption reaction rate. The inventors found that when based on the product component ratio, the step-activity α-[Zr(OH)4], β-[Zr4O2(OH) 12 ] and γ-[Zr4O4(OH)8] are introduced into the components as modifiers, which can effectively achieve long-term effects at a relatively low introduction amount, ultimately ensuring the stability of the product. At the same time, the product will not produce a large amount of mold scale during the injection molding process, and the production efficiency is high. At the same time, if the amount of zirconium hydroxide added is too high, the mechanical properties of the product will be affected. At the same time, the fluidity of the nylon material will increase during the injection molding process, and it will not be able to effectively and stably adsorb small molecules.

[0009] In addition, the inventors also found that if other substances with amphoteric properties (such as aluminum hydroxide) are selected as modifiers, not only will the amount of mold deposits generated fail to be reduced, but the mechanical properties of the product may even be weakened.

[0010] Preferably, the low mold deposit halogen-free flame retardant reinforced nylon material comprises the following components in parts by weight: 45-58 parts of nylon resin, 25-35 parts of glass fiber, 16-18 parts of halogen-free flame retardant, 0.2-0.5 parts of zirconium hydroxide and 0.8-2 parts of processing aid.

[0011] The introduction of nylon resin and glass fiber will affect the initial mechanical strength of the product, while the addition amount of halogen-free flame retardant will determine the probability of subsequent decomposition reaction. It needs to be matched with the addition amount of zirconium hydroxide. After screening, the low-module halogen-free flame retardant reinforced material prepared with the above ratio has better comprehensive effect.

[0012] It should be noted that, in the present invention, the content of the nylon resin in the low mold scale halogen-free flame retardant reinforced nylon material is not less than 30wt%, and the additive amount meets the raw material and production requirements of conventional nylon composite materials. Preferably, the α-[Zr(OH)4], β-[Zr4O2(OH) 12 The molar ratio of α-[Zr(OH)4]:β-[Zr4O2(OH)8] is 12 ]: γ-[Zr4O4(OH)8]=1: (0.2~0.4): (0.15~0.2).

[0013] As described above, due to the difference in the activities of the three isomers, the side reaction products generated during the entire preparation and production process of the product can be effectively fixed and eliminated. Under the above ratio, the total amount of mold deposit generated during the preparation and production injection molding process of the product is minimal.

[0014] Preferably, the ratio test method of the three isomers of zirconium hydroxide is as follows: the zirconium hydroxide is kept at 120°C in an oven to a constant weight, then heated to 550°C in an air atmosphere using a thermogravimetric analyzer and the composition ratio is determined according to the thermal weight loss zone and thermal weight loss rate; wherein α-[Zr(OH)4], β-[Zr4O2(OH) 12 The weight loss rates of γ-[Zr4O4(OH)8] and γ-[Zr4O4(OH)8] are 26-27%, 17.5-18.5% and 12-13%, respectively. At the same time, zirconium hydroxide can also be directly tested by XRD to obtain a spectrum, and then the component ratio can be statistically calculated using fitting software based on the differences in the characteristic peaks of the three isomers.

[0015] Preferably, the zirconium hydroxide has an average pore size of 2 to 4 nm and a particle size D50 of 25 to 35 μm.

[0016] Preferably, the nylon resin is at least one of adipic acid hexamethylenediamine copolymer and caprolactam copolymer.

[0017] Preferably, the average diameter of the glass fiber is 8 μm to 15 μm.

[0018] Preferably, the halogen-free flame retardant is a mixture of aluminum diethylphosphinate and melamine polyphosphate in a mass ratio of (2.5-3.5):1.

[0019] It should be noted that the halogen-free flame retardant of the present invention is not limited to the type mentioned above. Due to the beneficial effect of zirconium hydroxide introduced into the low mold deposit halogen-free flame retardant reinforced nylon material of the present invention, it also has a good effect on other types of halogen-free flame retardants and can effectively reduce the amount of mold deposit of the product.

[0020] Preferably, the processing aid is at least one of a lubricant and an antioxidant.

[0021] More preferably, the lubricant is at least one of a silicone lubricant, an amide lubricant, a stearic acid lubricant, and an ester lubricant, and the antioxidant is at least one of a hindered phenol antioxidant and a phosphite antioxidant.

[0022] Another object of the present invention is to provide a method for preparing the low mold scale halogen-free flame retardant reinforced nylon material, comprising the following steps:

[0023] The components except the glass fiber are mixed uniformly, and then added into the twin-screw extruder from the main feeding port, the glass fiber is added into the side feeding port, mixed and melt-extruded into granules, so as to obtain the low mold scale halogen-free flame retardant reinforced nylon material.

[0024] Preferably, the temperature of the melt extrusion is 240-270°C.

[0025] Due to its improved formula, the low-mold-scale halogen-free flame-retardant reinforced nylon material of the present invention does not need to be produced by adopting a special process, has simple operation steps, and can realize industrial large-scale production.

[0026] Another object of the present invention is to provide an electronic and electrical component made of the low mold scale halogen-free flame retardant reinforced nylon material of the present invention.

[0027] The low mold deposit halogen-free flame retardant reinforced nylon material of the present invention can significantly improve the stability of the product without significantly reducing the expected mechanical strength by introducing a small amount of special zirconium hydroxide without changing the basic formula or production process of the original nylon resin and reinforcing filler. The material is particularly suitable for preparing electronic and electrical parts with high requirements for flame retardancy, mechanical strength and stability. At the same time, the amount of mold deposit generated by the parts during the production process is low. According to tests, the amount of mold deposit of the low mold deposit halogen-free flame retardant reinforced nylon material of the present invention can be maintained within a range below 1.5 mg after continuous mold molding of the mold for 200 times, and the production efficiency is high, and the production benefits of the obtained electronic and electrical parts are high.

[0028] The beneficial effect of the present invention is that the present invention provides a low-mold-deposit halogen-free flame-retardant reinforced nylon material. The material introduces a special composition of inorganic zirconium hydroxide without changing the halogen-free flame-retardant component or the processing technology. The component can fix acidic substances and decomposed small molecular substances, and then react with the acidic substances generated by the decomposition of the halogen-free flame-retardant component through the three special components it contains, thereby ultimately avoiding the degradation of the nylon resin in the product, reducing the amount of mold deposit generated in the production injection molding process, and will not affect the tensile strength and flame retardant properties of the product. DETAILED DESCRIPTION

[0029] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by those of ordinary skill in the art without making creative work premise belong to the protection scope of the present invention. The experimental reagents and instruments involved in the implementation of the present invention, unless otherwise specified, are all commonly used common reagents and instruments.

[0030] Examples 1 to 11

[0031] The embodiments of the low mold deposit halogen-free flame retardant reinforced nylon material of the present invention, the components of the low mold deposit halogen-free flame retardant reinforced nylon material are shown in Table 1.

[0032] The preparation method of the product comprises the following steps:

[0033] The components except the glass fiber are mixed uniformly, and then added into the twin-screw extruder from the main feed port, the glass fiber is added into the side feed port, mixed and melt-extruded into granules, so as to obtain the low mold scale halogen-free flame retardant reinforced nylon material; the temperature of the melt extrusion is 240-270°C.

[0034] Comparative Examples 1 to 5

[0035] The difference between the comparative examples and the embodiments is only in the types and proportions of components, as shown in Table 2.

[0036] Among the components described in each embodiment and comparative example,

[0037] Nylon resin 1: hexamethylenediamine adipate copolymer, INVISTA Nylon Chemical Co., Ltd., PA66 U3600;

[0038] Nylon resin 2: caprolactam copolymer, Guangdong Xinhui Meida Nylon Co., Ltd., PA6 M2800;

[0039] Glass fiber: China Jushi Co., Ltd. produces 584 type fiber, with an average diameter of 11μm;

[0040] Halogen-free flame retardant 1: Compound: aluminum diethylphosphinate (Clariant Chemical Co., Ltd., OP-1230) and melamine polyphosphate (Budenheim, BUDIT 3141) are compounded in a mass ratio of 3:1;

[0041] Halogen-free flame retardant 2: melamine cyanurate (Sichuan Fine Chemical Design Institute, MCA-F);

[0042] Antioxidant: a mixture of commercially available hindered phenol antioxidant and phosphite antioxidant in a mass ratio of 1:1;

[0043] Lubricant: Commercially available silicone lubricant;

[0044] The zirconium hydroxides 1 to 3 and 5 are all from Jiangxi Jingan High-Tech Co., Ltd.;

[0045] Zirconium hydroxide 1: α-[Zr(OH)4]: β-[Zr4O2(OH) 12 ]: γ-[Zr4O4(OH)8]=1:0.3:0.18;

[0046] Zirconium hydroxide 2: α-[Zr(OH)4]: β-[Zr4O2(OH) 12 ]: γ-[Zr4O4(OH)8]=1:0.2:0.2;

[0047] Zirconium hydroxide 3: α-[Zr(OH)4]: β-[Zr4O2(OH) 12 ]: γ-[Zr4O4(OH)8]=1:0.4:0.15;

[0048] Zirconium hydroxide 4: α-[Zr(OH)4]: β-[Zr4O2(OH) 12 ]: γ-[Zr4O4(OH)8]=0.5:1:0.2;

[0049] Zirconium hydroxide 5: α-[Zr(OH)4]: β-[Zr4O2(OH) 12 ]: γ-[Zr4O4(OH)8]=1:0.5:0.1;

[0050] Zirconium hydroxide 6: α-[Zr(OH)4]: β-[Zr4O2(OH) 12 ]: γ-[Zr4O4(OH)8]=1:1:0;

[0051] Zirconium hydroxide 7: α-[Zr(OH)4]: β-[Zr4O2(OH) 12 ]: γ-[Zr4O4(OH)8]=1:0:0;

[0052] Aluminum hydroxide: Luoyang Zhongchao, AH-01DG.

[0053] Unless otherwise specified, the antioxidants and lubricants used in the various embodiments and comparative examples of the present invention are all commercially available raw materials, and the component raw materials used in each parallel experiment are all of the same kind. It should also be noted that the zirconium hydroxides 1 to 3 and 5 are actually commercially available products. Due to the difference in products between batches, the content ratio of isomers in the products is also different; while zirconium hydroxides 4, 6, and 7 are homemade products, using an acidic solution of a zirconium source to react in an ammonia environment, adjusting the pH of the solution to precipitate zirconium hydroxides of different crystal forms, and then grinding, sieving, and combining them, refer to the prior art "Preparation of Powdered Zirconium Hydroxide" - "Rare Metals Express" - Wang Zebin et al. The inventors used the isomer analysis method thermogravimetric method to confirm that the above-mentioned products with different proportions were implemented and tested in the embodiments / comparative examples; the average pore size of the zirconium hydroxide was 2 to 4 nm, and the particle size D50 was 25 to 35 μm. 。

[0054] Table 1

[0055]

[0056] Table 2

[0057]

[0058] Effect Example 1

[0059] In order to verify the performance of the product of the present invention, the following performance tests were performed on the products of each embodiment and comparative example. The specific steps are as follows:

[0060] (1) Mold deposit test: After each product is continuously injected 200 times at an injection molding temperature of 280-300°C, the mold deposit on the mold is collected and weighed;

[0061] (2) Tensile strength test: According to GB / T 1040.1-2018, the product was injection molded into a type I tensile specimen for testing. The test conditions were: tensile rate 10 mm / min;

[0062] (4) Flame retardant grade: According to GB / T 2408-2008 standard, the materials of the embodiments and comparative examples were subjected to vertical combustion performance test, the thickness of the test specimen was 0.8 mm, and the flame retardant grades were divided into V-0, V-1, V-2 and no grade.

[0063] The test results are shown in Tables 3 and 4.

[0064] Table 3

[0065]

[0066] Table 4

[0067]

[0068] As can be seen from Tables 3 and 4, the low mold scale halogen-free flame retardant reinforced nylon material described in each embodiment of the present invention is not only unaffected in tensile strength (still retaining more than 100MPa) and flame retardant properties compared to the original formula of the comparative example 1 product, but also the residual mold scale amount after 200 times of mold injection molding is reduced from 2.30mg of comparative example 1 to less than 1.5mg, indicating that the product effectively solves the decomposition of the flame retardant components of the existing products and the negative effects brought about, so that the product has better stability. According to the comparison of the products of Examples 1 to 5, when the product components are preferably: 45 to 58 parts of nylon resin, 25 to 35 parts of glass fiber, 16 to 18 parts of halogen-free flame retardant, 0.2 to 0.5 parts of zirconium hydroxide and 0.8 to 2 parts of processing aids, the comprehensive performance of the product is better. By comparing Example 1 with Examples 7 to 10 and Comparative Examples 3 to 5, it can be seen that when the zirconium hydroxide in the product is replaced with other similar hydroxide types, the product is not only difficult to achieve good stability, but also unable to solve the mold fouling problem, and may even affect the intrinsic tensile strength. When zirconium hydroxide is introduced, if the three isomers cannot be matched, the product is also difficult to achieve the expected effect; and when the ratio of the three isomers is maintained within the range of 1: (0.2 to 0.4): (0.15 to 0.2), the mold fouling of the product is the lowest. However, when the amount of zirconium hydroxide added is too much, as shown in Comparative Example 2, the performance of the product will decline.

[0069] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A low mold scale halogen-free flame retardant reinforced nylon material, It is characterized in that The composition comprises the following components in parts by weight: 40-60 parts of nylon resin, 20-40 parts of glass fiber, 14-20 parts of halogen-free flame retardant, 0.1-1 parts of zirconium hydroxide and 0.8-2 parts of processing aid; the zirconium hydroxide includes α-[Zr(OH) 4 ]、β-[Zr 4 O 2 (OH) 12 ] and γ-[Zr 4 O 4 (OH) 8 ]; the α-[Zr(OH) 4 ]、β-[Zr 4 O 2 (OH) 12 ] and γ-[Zr 4 O 4 (OH) 8 The molar ratio of α-[Zr(OH) 4 ]:β-[Zr 4 O 2 (OH) 12 ]:γ-[Zr 4 O 4 (OH) 8 ]=1:(0.2~0.4):(0.15~0.2).

2. The low mold fouling halogen-free flame retardant reinforced nylon material as claimed in claim 1, It is characterized in that The invention comprises the following components in parts by weight: 45-58 parts of nylon resin, 25-35 parts of glass fiber, 16-18 parts of halogen-free flame retardant, 0.2-0.5 parts of zirconium hydroxide and 0.8-2 parts of processing aid.

3. The low mold fouling halogen-free flame retardant reinforced nylon material as claimed in claim 1, It is characterized in that The nylon resin is at least one of adipic acid hexamethylenediamine copolymer and caprolactam copolymer.

4. The low mold fouling halogen-free flame retardant reinforced nylon material as claimed in claim 1, It is characterized in that The average diameter of the glass fiber is 8 μm to 15 μm.

5. The low mold fouling halogen-free flame retardant reinforced nylon material as claimed in claim 1, It is characterized in that The halogen-free flame retardant is a mixture of diethyl aluminum phosphinate and melamine polyphosphate in a mass ratio of (2.5-3.5):

1.

6. The low mold fouling halogen-free flame retardant reinforced nylon material as claimed in claim 1, It is characterized in that The processing aid is at least one of a lubricant and an antioxidant.

7. The method for preparing the low mold scale halogen-free flame retardant reinforced nylon material according to any one of claims 1 to 6, It is characterized in that The following steps are involved: The components except the glass fiber are mixed uniformly, and then added into the twin-screw extruder from the main feeding port, the glass fiber is added into the side feeding port, mixed and melt-extruded into granules, so as to obtain the low mold scale halogen-free flame retardant reinforced nylon material.

8. An electronic and electrical component made from the low mold scale halogen-free flame retardant reinforced nylon material according to any one of claims 1 to 6.