Preparation method of dumbbell-shaped gold-cerium oxide nanomaterial, its product and application
By preparing dumbbell-shaped gold-cerium oxide nanomaterials and utilizing their ability to generate oxygen and reactive oxygen species under light, the problem of poor targeting and hypoxic microenvironment of phototherapy and chemotherapy in the treatment of malignant tumors has been solved, and the treatment of malignant tumors has been achieved. Effective tumor suppression and immune activation reduce toxic and side effects during treatment.
Patent Information
- Application Number
- CN202310241797.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-14
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-03-14
AI Technical Summary
Existing phototherapy and chemotherapy have problems in the treatment of malignant tumors, such as poor targeting, high toxic and side effects, and a hypoxic microenvironment that affects the therapeutic effect. In particular, the photosensitizer's production efficiency of reactive oxygen species at the tumor site is low, and the treatment process is complex, which requires Combined with other adjuvants or immune checkpoint inhibitors.
Dumbbell-shaped gold-cerium oxide nanomaterials are prepared through a hydrothermal reaction. Their unique structural characteristics are used to generate oxygen and reactive oxygen species under light conditions, induce tumor immune-derived cell death, and improve the hypoxic microenvironment through oxygen evolution reaction. , to achieve the suppression of primary, distant and metastatic tumors.
It achieves effective tumor killing and immune activation under low-power light, reduces toxic side effects during treatment, does not require other adjuvants or immune checkpoint inhibitors, and has good biosafety and industrial production potential.
Smart Images

Figure CN116370625B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of preparation of gold-cerium oxide, and relates to a preparation method of a dumbbell-shaped gold-cerium oxide nano material, a product thereof and an application thereof. Background Art
[0002] For a long time, malignant tumors have seriously threatened human health. At present, the clinical tumor treatment model is still mainly surgical resection and chemotherapy. However, surgical resection is often accompanied by incomplete lesion resection, which often leads to tumor recurrence and metastasis; traditional small molecule chemotherapy drugs have problems such as poor targeting and short circulation time in the body, which makes it difficult to effectively enrich the tumor site. At the same time, its serious toxic side effects also affect the patient's treatment effect and health. In recent years, immunotherapy has made good progress in the treatment of malignant tumors. It can inhibit the primary tumor while mobilizing the body's immune system to achieve the inhibition of distal or metastatic tumors. However, the low immunogenicity of the tumor seriously affects its treatment efficiency. At the same time, the immunosuppressive microenvironment of the tumor site (such as hypoxia) also seriously reduces the effect of immunotherapy. Therefore, in view of the problem of low tumor immunogenicity, it is very important to develop new immunotherapy models, improve the tumor immunosuppressive microenvironment, and reduce the toxic side effects during treatment.
[0003] Phototherapy, including photothermal and photodynamic therapy, has received increasing attention in tumor treatment due to its good spatiotemporal controllability and low invasiveness. In addition, studies have found that phototherapy can induce immunogenic cell death in tumors by inducing phototherapeutic agents to produce reactive oxygen or excessive heat at the tumor site, thereby stimulating a series of immune processes in the body to achieve tumor treatment. However, the therapeutic effect of this type of photoimmunotherapy is also affected by the hypoxic immune microenvironment of the tumor, especially for photosensitizers, whose reactive oxygen production efficiency is heavily dependent on oxygen. The hypoxic microenvironment at the tumor site will first affect its reactive oxygen production efficiency. In addition, although all immunogenic cell death caused by photothermal therapy mainly depends on the excessive heat generated by photothermal materials under laser irradiation, the photothermal preparations reported so far often need to be irradiated with excessively high power lasers to produce sufficient photothermal effects. Therefore, the immune response induced by a single traditional optical therapy cannot achieve a good therapeutic effect. In order to achieve the good therapeutic effect of phototherapy in immunotherapy, that is, to effectively induce immunogenic cell death while improving the hypoxic tumor microenvironment, thereby triggering a strong immune response in the body, researchers have also made some attempts. For example, phototherapy agents are combined with oxygen-generating agents (such as manganese oxide, hemoglobin, and perfluorocarbons) in order to improve the hypoxic microenvironment of tumors. However, these composite materials often have complex preparation processes, or their oxygen production efficiency is affected by the concentration of hydrogen peroxide in the tumor area, and there are problems such as drug leakage during drug delivery. In addition, current phototherapy preparations often need to be used in combination with adjuvants or immune checkpoint inhibitors, which also increases the complexity, cost, and some safety issues of the treatment process.
[0004] Therefore, there is an urgent need to develop a simple phototherapeutic agent that not only has excellent tumor killing properties and can effectively induce tumor immunogenic cell death, but also can improve the tumor hypoxic microenvironment and achieve effective inhibition of primary tumors, distant tumors and metastases without the need to combine with other immune adjuvants or immune checkpoint inhibitors. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a dumbbell-shaped gold-cerium oxide nanomaterial. The prepared dumbbell-shaped gold-cerium oxide nanomaterial can be used in the preparation of tumor treatment drugs to effectively achieve photoimmunotherapy effects.
[0006] The technical solution provided by the present invention is:
[0007] The present invention provides a method for preparing a dumbbell-shaped gold-cerium oxide nanomaterial, the preparation method comprising the following steps:
[0008] S1, adding hexadecyltrimethylammonium bromide solution, potassium chloroplatinite solution, cerium acetate solution and double distilled water to the gold nanorod solution in sequence to obtain a mixed solution;
[0009] S2. The mixed solution in step S1 is subjected to a hydrothermal reaction to obtain dumbbell-shaped gold-cerium oxide nanomaterials (GCNRs).
[0010] In the present invention, due to the lattice structure and curvature difference of the gold rod, the density of hexadecyltrimethylammonium bromide at both ends of the gold rod is lower than that of hexadecyltrimethylammonium bromide at the side of the gold rod, and the two ends of the gold rod have smaller steric hindrance than the side, so the chloroplatinous acid ions will be preferentially adsorbed to the two ends of the gold rod. Subsequently, the cerium precursor (cerium acetate) will be hydrolyzed to generate cerium hydroxide under high temperature conditions, and then the chloroplatinous acid ions adsorbed on the surface of the gold rod are oxidized, nucleated, and grown to achieve selective site deposition of cerium oxide. The anisotropic structural feature makes it have good photocatalytic performance, can achieve dumbbell-shaped gold-cerium oxide nanomaterials effective electron-hole separation, can not only make the trivalent cerium and oxygen hole ratio of the cerium oxide surface under illumination conditions increase, improve the catalytic activity of cerium oxide itself, and can also produce oxygen by oxygen evolution reaction, which lays a chemical foundation for inducing tumor site-specific toxicity and improving its hypoxic microenvironment.
[0011] The dumbbell-shaped gold-cerium oxide nanomaterial has a long diameter of 132.57±19.78 nanometers and a short diameter of 23.23±7.32 nanometers. The size of the dumbbell-shaped gold-cerium oxide nanomaterial is conducive to being taken up by tumor cells, and does not show obvious toxicity after cell uptake. Due to its unique time-space separation structural characteristics, it can promote its reaction with hydrogen peroxide in the tumor site to generate highly toxic hydroxyl radicals (·OH) under near-infrared light irradiation, and at the same time generate toxic superoxide anions (·O2 - ), which is then converted into hydroxyl radicals and highly toxic singlet oxygen ( 1 O2), these reactive oxygen species can effectively promote tumor immunogenic cell death. At the same time, the dumbbell-shaped gold-cerium oxide nanomaterial can catalyze water into oxygen through the oxygen evolution reaction, effectively alleviating the tumor hypoxic microenvironment, achieving good regulation of its immunosuppressive microenvironment, and effectively achieving the effect of photoimmunotherapy.
[0012] The feeding ratio of the hexadecyltrimethylammonium bromide solution, potassium chloroplatinite solution, cerium acetate solution, double distilled water and gold nanorods in the present invention is 1-80 μg: 1-80 μg: 0.7-4.2 mg: 3-15 ml: 0.3-3 mg, so as to control the deposition position of cerium oxide on the surface of the gold rod. The concentrations of the hexadecyltrimethylammonium bromide solution, potassium chloroplatinite solution and cerium acetate solution are 0.1 mM, 0.1 mM and 10 mM respectively.
[0013] Preferably, the feeding ratio of the hexadecyltrimethylammonium bromide solution, potassium chloroplatinite solution, cerium acetate solution, double distilled water and gold nanorods is 2-60 μg: 0.5-20 μg: 0.3-3 mg: 3-12 ml: 0.4-2.3 mg.
[0014] The temperature of the hydrothermal reaction in the present invention is 80-130° C., and the reaction time is 1-5 h. Preferably, the temperature of the hydrothermal reaction is set to 100° C., and the reaction time is 1-4 h.
[0015] In the present invention, the major diameter of the gold nanorods is 87.23±12.34 nanometers, and the minor diameter is 23.37±4.28 nanometers.
[0016] In the present invention, the preparation method of gold nanorods can be: adding chloroauric acid and sodium borohydride to a hexadecyltrimethylammonium bromide solution, stirring and reacting to generate seed crystals for preparing gold nanorods; adding the seed crystals and chloroauric acid, silver nitrate, hydrochloric acid, and ascorbic acid to a hexadecyltrimethylammonium bromide solution, stirring and reacting to generate gold nanorods.
[0017] The preparation method of the dumbbell-shaped gold-cerium oxide nanomaterial of the present invention comprises: modifying the dumbbell-shaped gold-cerium oxide nanomaterial with an amphiphilic polymer ligand. By a ligand exchange method, the amphiphilic polymer ligand is replaced with surface hexadecyltrimethylammonium bromide to improve its colloidal stability and biocompatibility, and obtain a dumbbell-shaped gold-cerium oxide nanomaterial that can be well and stably dispersed in an aqueous phase.
[0018] Preferably, the amphiphilic polymer ligand is amphiphilic polymer polyethylene glycol.
[0019] Preferably, the amphiphilic polymer ligand is selected from alendronate-modified polyethylene glycol, thiol-polyethylene glycol, albumin, polyvinyl alcohol, pluronic, hyaluronic acid, polyethylene glycol-polylactic acid block copolymer, poloxamer, polyvinyl alcohol, alginate, sodium dodecyl sulfate, polyvinyl pyrrolidone and gelatin.
[0020] Preferably, the amphiphilic polymer ligand is selected from alendronate-modified polyethylene glycol and thiol-polyethylene glycol.
[0021] Preferably, the mass feed ratio of the dumbbell-shaped gold-cerium oxide nanomaterial to the amphiphilic polymer macromolecule is 1:1-50.
[0022] The modification of the amphiphilic polymer macromolecule in the present invention adopts the ligand exchange method.
[0023] Preferably, the ligand exchange method comprises: ultrafiltration and concentration of dumbbell-shaped gold-cerium oxide nanomaterials, adding them to an aqueous solution containing amphiphilic polymer macromolecules, stirring at room temperature overnight, and centrifugally resuspending to obtain bell-shaped gold-cerium oxide nanomaterials with biocompatibility.
[0024] The present invention also provides a dumbbell-shaped gold-cerium oxide nanomaterial prepared by the above-mentioned preparation method.
[0025] The present invention also provides a use of the dumbbell-shaped gold-cerium oxide nanomaterial in preparing drugs for treating tumors.
[0026] Furthermore, the dumbbell-shaped gold-cerium oxide nanomaterial is used in the preparation of drugs for inhibiting primary tumors and distal tumors.
[0027] The dumbbell-shaped gold-cerium oxide nanomaterial provided by the present invention is used for anti-tumor application by utilizing its photocatalytic activity under near-infrared light excitation, and can effectively treat proximal and distal tumors under near-infrared light excitation.
[0028] By precisely controlling the deposition position of the cerium oxide nanosheets on the gold rod, the separation rate of hot electrons and holes under near-infrared light excitation is significantly improved. The resulting bell-shaped gold-cerium oxide nanomaterial has good photocatalytic properties, can effectively oxidize the substrate to generate reactive oxygen under illumination conditions, and produce oxygen through oxygen evolution reaction. With this characteristic, by administering drugs and laser irradiation at the primary tumor site, the material can produce reactive oxygen at the primary tumor site to induce tumor immunogenic cell death while alleviating tumor hypoxia through oxygen evolution reaction, thereby activating the subsequent immune response process, and the primary tumor can be ablated under in situ administration and illumination conditions to achieve effective inhibition of primary tumors, distal tumors and metastatic tumors, with good tumor inhibition effects. And the dumbbell-shaped gold-cerium oxide nanomaterial provided by the present invention has good biosafety under non-illumination conditions.
[0029] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0030] (1) The preparation conditions of the present invention are mild and controllable, with extremely high repeatability, very low cost, and good industrial production and clinical transformation potential.
[0031] (2) The dumbbell-shaped gold-cerium oxide nanomaterial prepared in the present invention has temporal and spatial separation, can effectively separate electrons and holes under illumination conditions, and has good photocatalytic performance. In addition, the dumbbell-shaped gold-cerium oxide nanomaterial prepared in the present invention also has good photothermal conversion performance, and can achieve tumor treatment by inducing hyperthermia.
[0032] (3) The dumbbell-shaped gold-cerium oxide nanomaterial prepared in the present invention can induce the generation of reactive oxygen species under near-infrared light irradiation, thereby achieving effective primary tumor ablation and immunogenic cell death. At the same time, it can effectively alleviate tumor hypoxia through the oxygen evolution reaction, effectively induce the body's immune activation, and has good spatiotemporal controllability. It does not have cytotoxicity under non-light conditions, and therefore has good biosafety and selectivity.
[0033] (4) The dumbbell-shaped gold-gold-cerium oxide nanomaterial prepared in the present invention has excellent photocatalytic performance and can be used under low-power light (300mW cm -2 ) to achieve effective photocatalytic tumor killing.
[0034] (5) The dumbbell-shaped gold-gold-cerium oxide nanomaterial prepared in the present invention can effectively induce the body's immune response. Only by administering the dumbbell-shaped gold-gold-cerium oxide nanomaterial alone, it is possible to kill the primary tumor, distal tumor and metastatic tumor without combining with other adjuvants or immune checkpoint inhibitors. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 TEM image of the dumbbell-shaped gold-cerium oxide nanomaterial prepared in Example 1;
[0036] Figure 2 This is the XPS image of the dumbbell-shaped gold-cerium oxide nanomaterial prepared in Example 1;
[0037] Figure 3 This is the XRD pattern of the dumbbell-shaped gold-cerium oxide nanomaterial prepared in Example 1;
[0038] Figure 4 TA curve diagram of dumbbell-shaped gold-cerium oxide nanomaterial prepared in Example 1;
[0039] Figure 5 This is a graph evaluating the efficiency of the dumbbell-shaped gold-cerium oxide nanomaterial in Example 1 in generating active oxygen under no light conditions;
[0040] Figure 6 This is a graph evaluating the efficiency of the dumbbell-shaped gold-cerium oxide nanomaterial in Example 1 in generating active oxygen under near-infrared light conditions;
[0041] Figure 7 This is the oxygen production diagram of the dumbbell-shaped gold-cerium oxide nanomaterial in Example 1;
[0042] Figure 8 This is a diagram for evaluating the cytotoxicity of the dumbbell-shaped gold-cerium oxide nanomaterial in Example 1 to tumor cells under non-illumination and near-infrared light irradiation;
[0043] Fig. 9 This is a diagram for evaluating the tumor inhibition effect of the dumbbell-shaped gold-cerium oxide nanomaterial on primary tumors under near-infrared light irradiation in Example 1;
[0044] Fig.10 This is a diagram for evaluating the tumor inhibition effect of the dumbbell-shaped gold-cerium oxide nanomaterial on distal tumors under near-infrared light irradiation in Example 1;
[0045] Fig.11 This is a diagram evaluating the tumor inhibition effect of the dumbbell-shaped gold-cerium oxide nanomaterial on lung metastases under near-infrared light irradiation in Example 1. DETAILED DESCRIPTION
[0046] The present invention is described in detail below with reference to the embodiments.
[0047] In the following examples, the gold nanorods used were prepared by the following method:
[0048] Dissolve 6.7 mg of sodium borohydride in 10 ml of ice water to prepare a sodium borohydride solution. Mix 1.95 ml of CTAB aqueous solution (0.1 M) and 50 μl of tetrahydrate chloroauric acid aqueous solution (10 mM), and stir in a 27°C water bath to obtain a mixed solution A. Subsequently, add the above-prepared 50 μl of sodium borohydride aqueous solution to the mixed solution A, stir in a 27°C water bath for 2 min, and then let stand for 2 h to obtain a gold seed solution for use. Subsequently, 15 ml of tetrahydrate chloroauric acid aqueous solution (10 mM), 7.5 ml of silver nitrate aqueous solution (4 mM), 6 ml of hydrochloric acid (1 M), 2.4 ml of ascorbic acid aqueous solution (0.1 mM) and 450 μl of the gold seed solution prepared above were added to 300 mL of CTAB aqueous solution (0.1 M) in sequence, stirred for 2 min in a 27 ° C water bath, and then allowed to stand for at least 1.5 h, followed by centrifugation (10000 rpm, 15 min), the supernatant was discarded, and then double distilled water was added for centrifugal washing once (10000 rpm, 15 min), and the centrifugal product was resuspended and dispersed in double distilled water to obtain a gold nanorod stock solution. The prepared gold nanorods have a long diameter of about 87 nm and a transverse diameter of about 23 nm.
[0049] Example 1
[0050] (1) 40 μg of hexadecyltrimethylammonium bromide solution (0.1 mM), 5 μg of potassium chloroplatinite solution (0.1 mM), and 2 mg of cerium acetate solution (10 mM) were sequentially added to an aqueous solution containing 2 mg of gold nanorods, the volume was made up to 15 ml with double distilled water, and the mixture was gently shaken to obtain a mixed solution;
[0051] (2) The mixed solution in step (1) was transferred to a high-temperature hydrothermal reactor and reacted at 100° C. for 1 h. The reaction system was then cooled to room temperature and the precipitate was collected by centrifugation to obtain a dumbbell-shaped gold-cerium oxide nanomaterial (GCNRs). The product was collected and dispersed in distilled water.
[0052] The dumbbell-shaped gold-cerium oxide nanomaterials were characterized by TEM, XPS and XRD. Figure 1 As shown in Figure 2, the synthesized gold-cerium oxide nanomaterial is in a dumbbell shape, and the cerium oxide nanosheets are selectively deposited on both ends of the gold rod. The gold-cerium oxide nanomaterial is in a dumbbell shape with a long diameter of 132.57±19.78 nanometers and a short diameter of 23.23±7.32 nanometers. XPS characterization is as follows Figure 2 As shown in Figure 2, trivalent cerium and tetravalent cerium coexist in the dumbbell-shaped gold-cerium oxide nanomaterial. Figure 3 As shown, the gold rod and cerium oxide show strong diffraction peaks, and the dumbbell-shaped gold-cerium oxide nanomaterial has a polycrystalline structure.
[0053] (3) The dumbbell-shaped gold-cerium oxide nanomaterial was added to a mixed aqueous solution of thiol-polyethylene glycol polymer and alenphosphate-modified polyethylene glycol polymer (1:10:10, g / g), stirred at room temperature for 12 h for surface ligand exchange, and then centrifuged to wash away excess surface ligands.
[0054] Example 2
[0055] (1) 40 μg of hexadecyltrimethylammonium bromide solution (0.1 mM), 5 μg of potassium chloroplatinite (0.1 mM), and 2 mg of cerium acetate solution (10 mM) were added sequentially to an aqueous solution containing 2 mg of gold nanorods, the volume was made up to 15 ml with double distilled water, and the mixed solution was gently shaken to obtain a uniform solution.
[0056] (2) The mixed solution in step (1) was transferred to a high-temperature hydrothermal autoclave and reacted at 100° C. for 3 h. The reaction system was then cooled to room temperature and the precipitate was collected by centrifugation to obtain a dumbbell-shaped gold-cerium oxide nanomaterial (GCNRs). The product was collected and dispersed in distilled water.
[0057] The dumbbell-shaped gold-cerium oxide nanomaterials were characterized by TEM, XPS and XRD. The synthesized gold-cerium oxide nanomaterials were dumbbell-shaped, and cerium oxide nanosheets were selectively deposited on both ends of the gold rod. The dumbbell-shaped gold-cerium oxide nanomaterials had a long diameter of 132.57±19.78 nanometers and a short diameter of 23.23±7.32 nanometers. XPS showed that trivalent cerium and tetravalent cerium coexisted in the dumbbell-shaped gold-cerium oxide nanomaterials. XRD showed that the gold rod and cerium oxide showed strong diffraction peaks, and the dumbbell-shaped gold-cerium oxide nanomaterials had a polycrystalline structure.
[0058] (3) The dumbbell-shaped gold-cerium oxide nanomaterial was added to a mixed aqueous solution of thiol-polyethylene glycol polymer and alenphosphate-modified polyethylene glycol polymer (1:10:10, g / g), stirred at room temperature for 12 h for surface ligand exchange, and then centrifuged to wash away excess surface ligands.
[0059] Example 3
[0060] (1) 5 μg of hexadecyltrimethylammonium bromide solution (0.1 mM), 20 μg of potassium chloroplatinite solution (0.1 mM), and 2 mg of cerium acetate solution (10 mM) were added sequentially to an aqueous solution containing 2 mg of gold nanorods, the volume was made up to 15 ml with double distilled water, and the mixed solution was shaken gently to obtain a uniform solution.
[0061] (2) The mixed solution in step (1) was transferred to a high-temperature hydrothermal reactor and reacted at 100° C. for 1 h. The reaction system was then cooled to room temperature and the precipitate was collected by centrifugation to obtain a dumbbell-shaped gold-cerium oxide nanomaterial (GCNRs). The product was collected and dispersed in distilled water.
[0062] The dumbbell-shaped gold-cerium oxide nanomaterials were characterized by TEM, XPS and XRD. The synthesized gold-cerium oxide nanomaterials were dumbbell-shaped, and cerium oxide nanosheets were selectively deposited on both ends of the gold rod. The dumbbell-shaped gold-cerium oxide nanomaterials had a long diameter of 132.57±19.78 nanometers and a short diameter of 23.23±7.32 nanometers. XPS showed that trivalent cerium and tetravalent cerium coexisted in the dumbbell-shaped gold-cerium oxide nanomaterials. XRD showed that the gold rod and cerium oxide showed strong diffraction peaks, and the dumbbell-shaped gold-cerium oxide nanomaterials had a polycrystalline structure.
[0063] (3) The dumbbell-shaped gold-cerium oxide nanomaterial was added to a mixed aqueous solution of thiol-polyethylene glycol polymer and alenphosphate-modified polyethylene glycol polymer (1:10:10, g / g), stirred at room temperature for 12 h for surface ligand exchange, and then centrifuged to wash away excess surface ligands.
[0064] Example 4
[0065] (1) 40 μg of hexadecyltrimethylammonium bromide solution (0.1 mM), 5 μg of potassium chloroplatinite solution (0.1 mM), and 2 mg of cerium acetate solution (10 mM) were added sequentially to an aqueous solution containing 2 mg of gold nanorods, the volume was made up to 15 ml with double distilled water, and the mixed solution was shaken gently to obtain a uniform solution.
[0066] (2) The mixed solution in step (1) was transferred to a high-temperature hydrothermal reactor and reacted at 100° C. for 1 h. The reaction system was then cooled to room temperature and the precipitate was collected by centrifugation to obtain a dumbbell-shaped gold-cerium oxide nanomaterial (GCNRs). The product was collected and dispersed in distilled water.
[0067] The dumbbell-shaped gold-cerium oxide nanomaterials were characterized by TEM, XPS and XRD. The synthesized gold-cerium oxide nanomaterials were dumbbell-shaped, and cerium oxide nanosheets were selectively deposited on both ends of the gold rod. The dumbbell-shaped gold-cerium oxide nanomaterials had a long diameter of 132.57±19.78 nanometers and a short diameter of 23.23±7.32 nanometers. XPS showed that trivalent cerium and tetravalent cerium coexisted in the dumbbell-shaped gold-cerium oxide nanomaterials. XRD showed that the gold rod and cerium oxide showed strong diffraction peaks, and the dumbbell-shaped gold-cerium oxide nanomaterials had a polycrystalline structure.
[0068] (3) The dumbbell-shaped gold-cerium oxide nanomaterial was added to a mixed aqueous solution of thiol-polyethylene glycol polymer and alenphosphate-modified polyethylene glycol polymer (1:20:20, g / g), stirred at room temperature for 48 h for surface ligand exchange, and then centrifuged to wash away excess surface ligands.
[0069] Performance test
[0070] (1) Evaluation of photogenerated carrier dynamics
[0071] The generation and attenuation of carriers in dumbbell-shaped gold-cerium oxide nanomaterials were detected by transient absorption spectroscopy. Figure 4 As shown, the photoexcited carriers tend to decay as time goes by.
[0072] (2) Evaluation of active oxygen generation performance Evaluation of active oxygen in vitro
[0073] (2.1) Dumbbell-shaped gold-cerium oxide nanomaterial (prepared in Example 1, 5 μg), 10 μl H2O2 solution (2M), and 10 μl TMB dimethyl sulfoxide solution (100 mM) were dispersed in acetic acid / sodium acetate buffer (2 mL, pH = 5.0).
[0074] The oxidation of TMB by active oxygen generated by dumbbell-shaped gold-cerium oxide nanomaterials at different time periods (1, 3, 5, 7, 10, 15 and 20 min) was detected by UV-visible spectroscopy. Figure 5 As shown, the absorbance of TMB increases slowly with time, indicating that the dumbbell-shaped gold-cerium oxide nanomaterial itself has a certain oxidation activity and can induce the production of reactive oxygen species.
[0075] (2.2) Dumbbell-shaped gold-cerium oxide nanomaterial (prepared in Example 1, 5 μg), 10 μl H2O2 solution (2M), and 10 μl TMB dimethyl sulfoxide solution (100 mM) were dispersed in acetic acid / sodium acetate buffer (2 mL, pH = 5.0).
[0076] The oxidation of TMB by reactive oxygen species generated by dumbbell-shaped gold-cerium oxide nanomaterials under light conditions at different time periods (1, 3, 5, 7, 10, 15 and 20 min) was detected by UV-visible spectroscopy. Figure 6 As shown, the absorbance of TMB increased sharply with time, indicating that light irradiation can significantly enhance the generation of reactive oxygen species induced by dumbbell-shaped gold-cerium oxide nanomaterials.
[0077] (2.3) By comparison Figure 5 and 6 In comparison, light can promote the generation of hot electrons and holes in dumbbell-shaped gold-cerium oxide nanomaterials, among which hot electrons can promote the generation of trivalent cerium and oxygen holes, significantly improving their oxidation performance and active oxygen yield.
[0078] (3) Oxygen evolution reaction evaluation
[0079] The dumbbell-shaped gold-cerium oxide nanomaterial obtained in Example 1 was dispersed in water to obtain a dumbbell-shaped gold-cerium oxide nanomaterial aqueous solution (5 μg / ml) of a certain concentration. The oxygen content in the aqueous solution was measured with an oxygen meter under illumination and non-illumination conditions. The results are as follows: Figure 7 As shown, in the absence of light, the dumbbell-shaped gold-cerium oxide nanomaterial does not produce oxygen; however, under near-infrared light irradiation, the dumbbell-shaped gold-cerium oxide nanomaterial can effectively produce oxygen through oxygen evolution reaction.
[0080] (4) Cytotoxicity evaluation on breast cancer cell lines
[0081] Breast cancer cell line (4T1 cells) in logarithmic growth phase was taken and 1×10 4The cells were inoculated into a 96-well plate (200 μl / well) with 1640 culture medium containing 10% fetal bovine serum at a cell density of 10 cells / ml, and cultured in an incubator at 37°C and 5% CO2. After the cells were cultured for 12 hours, the culture medium was replaced with a culture medium containing dumbbell-shaped gold-cerium oxide nanomaterials (prepared according to the method of Example 1), wherein the concentration of the Au content was 0, 0.61, 1.23, 2.45, 4.9 and 9.8 μg / ml, respectively. After continuing to culture for 20 hours, the old culture medium was aspirated and washed once with PBS buffer. Then, MTT solution (200 μl / well) was added to the wells and incubated in a 37°C, 5% CO2 incubator for 1 to 4 h. Then, the MTT solution was aspirated and 200 μl DMSO solution was added. After the system was shaken and evenly mixed, the optical density OD value was measured on a microplate reader. For the light group, 4T1 cells in the logarithmic growth phase were taken and 1×10 4 The cells were inoculated into a 96-well plate (200 μl / well) with 1640 culture medium containing 10% fetal bovine serum at a cell density of 10 cells / ml, and cultured in an incubator at 37°C and 5% CO2. After the cells were cultured for 12 hours, the culture medium was replaced with a culture medium containing dumbbell-shaped gold-cerium oxide nanomaterials (prepared according to the method of Example 1), wherein the concentration of the Au content was 0, 0.61, 1.23, 2.45, 4.9 and 9.8 μg / ml, respectively. After 8 hours of culture, the old culture medium was aspirated and washed once with PBS buffer. Then, the cells in each well were irradiated with near-infrared light (808 nm, 5 min), and the cells were cultured for 12 h. Then, MTT solution (200 μl / well) was added to the wells and incubated in an incubator at 37°C, 5% CO2 for 1 to 4 h. Then, the MTT solution was aspirated, 200 μl DMSO solution was added, the system was shaken and the optical density OD value was measured on a microplate reader.
[0082] Data processing: Use the corresponding software of the microplate reader to process the data, calculate the average OD value of the four wells of each sample, and use the average value to calculate the cell viability (Cell Viability %) according to the following formula.
[0083] Cell Viability % = average OD value of sample group / average OD value of blank control group × 100% (Cell Viability % = OD sample / OD control ×100%)
[0084] Results Figure 8 .Depend on Figure 8The analysis showed that the dumbbell-shaped gold-cerium oxide nanomaterial had no obvious cytotoxicity under the condition of no light, but showed concentration-dependent cytotoxicity after light exposure. Therefore, after being taken up by tumor cells, the dumbbell-shaped gold-cerium oxide nanomaterial can produce obvious cytotoxicity under light exposure, but is relatively safe under the condition of no light.
[0085] (5) Evaluation of tumor inhibition effect
[0086] Twenty BALB / c mice were placed with tumors on the left and right sides of their backs to construct primary tumor and distal tumor models, and randomly divided into 4 groups, 5 mice in each group, including PBS (non-illumination group), PBS (illumination group), dumbbell-shaped gold-cerium oxide nanomaterials (prepared according to the method of Example 1) (non-illumination group) and dumbbell-shaped gold-cerium oxide nanomaterials (prepared according to the method of Example 1) (illumination group), for intratumoral administration. For the illumination group, near-infrared laser irradiation was given for 5 minutes after administration. The tumor volume (V) of the primary tumor and metastatic tumor was measured every other day, and the calculation formula was: V = L × W 2 / 2, W and L are the widest and longest diameters of the tumor, respectively. The tumor volume was calculated to monitor the tumor inhibition effect.
[0087] The results are as follows Fig. 9 and 10 The dumbbell-shaped gold-cerium oxide nanomaterial can significantly inhibit the growth of primary tumors under light conditions, and also has a good inhibitory effect on distal tumors. Fig.11 As shown, the dumbbell-shaped gold-cerium oxide nanomaterial can effectively inhibit the lung metastasis of tumors after irradiation, and has a good inhibitory effect on primary tumors, distant tumors and metastatic tumors.
[0088] The above-described embodiments provide a detailed description of the technical solutions and beneficial effects of the present invention. It should be understood that the above descriptions are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, supplements and equivalent substitutions made within the scope of the principles of the present invention should be included in the protection scope of the present invention.
Claims
1. Application of a dumbbell-shaped gold-cerium oxide nanomaterial in the preparation of drugs for treating tumors. It is characterized in that The preparation method of the dumbbell-shaped gold-cerium oxide nanomaterial comprises the following steps: S1. 40 µg of hexadecyltrimethylammonium bromide solution, 5 µg of potassium chloroplatinite solution, and 2 mg of cerium acetate solution were sequentially added to an aqueous solution containing 2 mg of gold nanorods, and the volume was fixed to 15 ml with double distilled water to obtain a mixed solution; the concentrations of hexadecyltrimethylammonium bromide solution, potassium chloroplatinite solution, and cerium acetate solution were 0.1 mM, 0.1 mM, and 10 mM, respectively; S2, subjecting the mixed solution in step S1 to a hydrothermal reaction to obtain a dumbbell-shaped gold-cerium oxide nanomaterial; The gold nanorod has a long diameter of 87 nm and a transverse diameter of 23 nm; the dumbbell-shaped gold-cerium oxide nanomaterial has a long diameter of 132.57 ± 19.78 nm and a short diameter of 23.23 ± 7.32 nm; The temperature of the hydrothermal reaction is 80-130°C, and the reaction time is 1-5 h; The application is for preparing a drug for treating and inhibiting lung metastasis of a tumor, and the tumor is breast cancer.
2. The use according to claim 1, It is characterized in that The preparation method further comprises modifying the dumbbell-shaped gold-cerium oxide nanomaterial with amphiphilic polymer polyethylene glycol.
3. The use according to claim 2, It is characterized in that The mass feed ratio of the dumbbell-shaped gold-cerium oxide nanomaterial to the amphiphilic polymer polyethylene glycol is 1:1-50.
4. The use according to claim 2, It is characterized in that The modification adopts the ligand exchange method; the amphiphilic polymer polyethylene glycol is selected from thiol-polyethylene glycol or alendronate-modified polyethylene glycol.