A method for treating organic pollutants using Fe-NC single-atom catalysts
Through the reduction and hydrogenation reaction between Fe-N-C single-atom catalyst and NaBH4, the Fe-Nx site adsorption and activation of BH4- is solved, and the existing catalysts are insufficient in catalytic reduction and hydrogenation are realized. Efficient removal, stability and wide applicability.
Patent Information
- Application Number
- CN202211686074.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-12-27
AI Technical Summary
The existing Fe-N-C catalysts have problems such as small specific surface area, few active sites and poor stability in catalytic reduction hydrogenation, making it difficult to quickly and thoroughly remove nitroaromatic organic pollutants in water.
The reduction and hydrogenation reaction was carried out by mixing Fe-N-C single-atom catalyst with NaBH4 for reduction and hydrogenation reaction. BH4- and nitrophenol were adsorbed through Fe-Nx active site, activate the B-H bond to generate·H, and achieve efficient reduction of paranitrophenol. The catalyst is dissolved from zinc salt and iron phthalocyanine in methanol to form a FePc@ZIF-8 precursor. After pyrolysis and acid solution treatment, Fe-N-C single atoms with rich Fe-Nx sites and mesoporous structures are prepared. catalyst.
It achieves rapid and thorough removal of paranitrophenol, has a high reaction rate, stable catalyst, wide pH range, low cost, and is suitable for industrial production.
Smart Images

Figure CN116371439B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalytic reduction, relates to a method for reducing organic pollutants, and specifically relates to a method for treating organic pollutants using Fe-NC single-atom catalysts. Background Art
[0002] Nitroaromatic hydrocarbons, including nitrophenols and some azo dyes, are dangerous organic pollutants present in industrial and agricultural production. They are widely used in industries such as leather, plastics, pharmaceuticals, pesticides and papermaking, causing serious damage to the water environment. In addition, nitroaromatic hydrocarbons are difficult to completely remove from water due to their strong light and heat stability and are not easily biodegradable. If they accumulate for a long time, they will cause damage to the human body. Therefore, it is necessary to find a simple and effective method to remove nitrophenols in water.
[0003] The catalytic hydrogenation method uses a catalyst to activate the hydrogen donor to produce a large amount of ·H, and then uses ·H to achieve the catalytic reduction of p-nitrophenol. Since the hydrogenation product aminophenol is less toxic and easier to mineralize than nitrophenol, and can be used as a chemical intermediate in the production of drugs, dyes, corrosion inhibitors, agricultural chemicals and imaging agents, it brings economic benefits. Therefore, catalytic hydrogenation is the most popular method for removing nitrophenol.
[0004] Previous studies have shown that noble metal nanoparticles such as platinum, gold and silver nanoparticles (Pt, Au and Ag NPs) homogeneous and heterogeneous catalysts are highly efficient catalysts for the hydrogenation of nitroaromatics. However, their high prices inevitably limit their industrial production and widespread application, so it is necessary to develop non-noble metal-based catalysts with good catalytic performance for the hydrogenation of nitroaromatics. Studies have demonstrated the catalytic activity of non-noble metal catalysts such as CuFe2O4, Co / SiO2, Cu / CuO / C, and Ni / SiO in the reduction of nitroaromatics, but the catalytic rate and catalyst stability still need to be further improved.
[0005] In recent years, metal nitrogen-doped carbon (MNC) catalysts have been regarded as good substitutes for precious metal catalysts and have attracted more and more attention due to their excellent catalytic performance in various reactions. However, the existing iron nitrogen-doped carbon (Fe-NC) catalysts are mainly used in electrocatalytic carbon dioxide reduction, electrocatalytic oxygen reduction, organic synthesis, persulfate activation, etc., and there are no reports on the application of Fe-NC catalysts in catalytic reduction hydrogenation to treat nitrophenol wastewater. In addition, the existing Fe-NC catalysts still have the following defects: small specific surface area and few active sites, which makes it difficult for the catalytic activity of Fe-NC catalysts to meet the requirements and is not conducive to the rapid removal of nitroaromatics. In addition, the conventional preparation method is also prone to the defects of iron atoms agglomerating to form clusters or particles, which will reduce the catalytic efficiency of the catalyst. Obviously, the existence of the above problems makes it difficult for Fe-NC catalysts to quickly and thoroughly destroy the BH bonds in NaBH4, so it is difficult to activate NaBH4 to produce a large amount of ·H, and it is difficult to reduce organic pollutants to low-toxic substances. Therefore, obtaining a Fe-NC single-atom catalyst with a large specific surface area, multiple active sites, high catalytic activity, and good stability is of great significance for effectively activating NaBH4 and achieving rapid and thorough removal of organic pollutants. Summary of the invention
[0006] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a method for treating organic pollutants using Fe-NC single atom catalyst with simple operation, high efficiency and good economic benefits.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0008] A method for treating organic pollutants using Fe-NC single-atom catalysts comprises the following steps:
[0009] The Fe-NC single atom catalyst is mixed with water containing organic pollutants, and NaBH4 is added to carry out reduction hydrogenation reaction to complete the treatment of organic pollutants in the water.
[0010] The above method is further improved, wherein the initial ratio of the Fe-NC single atom catalyst to the organic pollutant is 5 mg: 0.01 mmol to 0.05 mmol; and the molar ratio of NaBH4 to the organic pollutant is 1 to 16: 0.01 to 0.05.
[0011] The above method is further improved, wherein the organic pollutants in the water body containing organic pollutants are at least one of nitrophenol organic pollutants and dye organic pollutants; the nitrophenol organic pollutants are at least one of 2-nitrophenol, 4-nitrophenol, and 2,4-dinitrophenol; the dye organic pollutants are at least one of Congo red and chrome black T; the initial concentration of organic pollutants in the water body containing organic pollutants is 0.1mmol / L~0.5mmol / L; the pH of the water body containing organic pollutants is 3~11.
[0012] The above method is further improved in that the mixing is carried out under stirring conditions, and the stirring time is 30 minutes; the rotation speed is controlled to be 400r / min to 500r / min during the reduction hydrogenation reaction; and the time of the reduction hydrogenation reaction is controlled to be 3min to 25min.
[0013] The above method is further improved, wherein the Fe-NC single atom catalyst comprises an iron atom and a three-dimensional nitrogen-doped carbon skeleton; the iron atom exists in the form of a single atom; the iron atom coordinates with the nitrogen atom of the three-dimensional nitrogen-doped carbon skeleton to form an Fe-N site; the Fe-N site is dispersed on the three-dimensional nitrogen-doped carbon skeleton; and the total iron content in the Fe-NC single atom catalyst is 1.1wt% to 1.8wt%.
[0014] The above method is further improved in that the total iron content in the Fe-NC single-atom catalyst is 1.3wt% to 1.5wt%.
[0015] The above method is further improved in that the total iron content in the Fe-NC single-atom catalyst is 1.35wt%.
[0016] The above method is further improved, wherein the iron atom in the Fe-NC single atom catalyst is divalent; the carbon component in the three-dimensional nitrogen-doped carbon skeleton mainly exists in the form of amorphous carbon; the nitrogen atoms in the Fe-NC single atom catalyst also exist in the form of at least one of pyridinic nitrogen, pyrrolic nitrogen, graphitic nitrogen, and nitrogen oxide; the Fe-NC single atom catalyst has a hollow mesoporous structure; the Fe-NC single atom catalyst has a prismatic dodecahedral structure; the particle size of the Fe-NC single atom catalyst is 40nm to 120nm; the specific surface area of the Fe-NC single atom catalyst is 838.39m 2 / g~879.14m 2 / g.
[0017] The above method is further improved, wherein the Fe-NC single atom catalyst is prepared by the following method:
[0018] S1. Dissolve zinc salt and iron phthalocyanine in methanol at a mass ratio of 146.9:5 to form solution A; dissolve 2-methylimidazole in methanol to form solution B;
[0019] S2, adding solution A to solution B and stirring;
[0020] S3, washing and drying the product obtained after stirring to obtain a FePc@ZIF-8 precursor;
[0021] S4, pyrolyzing the FePc@ZIF-8 precursor;
[0022] S5. Soaking the pyrolysis product in an acid solution, washing, and drying to obtain an atomically dispersed Fe-NC catalyst.
[0023] The above method is further improved, wherein in S1, in solution A, the ratio of zinc salt to methanol is 14.69 mg:1 mL; the zinc salt is Zn(NO3)2·6H2O; in solution B, the ratio of 2-methylimidazole to methanol is 810.6 mg:50 mL; and the molar ratio of the zinc salt to 2-methylimidazole is 4:1.
[0024] The above method is further improved, wherein in S2, the stirring is carried out at a temperature of 60° C. and the stirring time is 24 hours.
[0025] The above method is further improved, in S3, the product is washed with methanol; the number of washings is 3 times; the drying is carried out under vacuum conditions; the drying temperature is 70°C.
[0026] The above method is further improved, wherein in S4, the pyrolysis is carried out under a nitrogen atmosphere; the heating rate during the pyrolysis is 2°C min -1 ; The pyrolysis is to heat the FePc@ZIF-8 precursor to 900°C for calcination; the calcination time is 2h to 3h.
[0027] The above method is further improved, wherein in S5, the acid solution is a non-oxidizing strong acid solution; the non-oxidizing strong acid solution is a sulfuric acid solution or a hydrochloric acid solution; the concentration of the acid solution is 0.5 mM; the soaking time is 24 h; the washing liquid used for washing is ultrapure water; the drying is carried out under vacuum conditions; and the drying temperature is 70°C.
[0028] Compared with the prior art, the advantages of the present invention are:
[0029] (1) The present invention provides a method for treating organic pollutants using Fe-NC single-atom catalysts, wherein the Fe-NC single-atom catalyst is used as a catalyst for activating NaBH4, and the Fe-NC single-atom catalyst, NaBH4, and water containing organic pollutants are mixed for hydrogenation reduction catalytic treatment, thereby achieving effective removal of organic pollutants and converting organic pollutants into chemical intermediates with high economic benefits and non-toxicity. The method has the advantages of simple operation, good economic benefits, easy recycling, high catalytic efficiency, wide pH application range, good recycling performance, etc., and can be widely used in treating organic pollutants (such as nitrophenols and azo dyes), which is of great significance for waste resource utilization and sustainable development. Taking 4-nitrophenol (4-NP) as an example, in the presence of NaBH4, the Fe-NC single-atom catalyst can be used to remove organic pollutants. x Active sites generate a large amount of ·H, thereby realizing the hydrogenation reduction of organic pollutants. The specific process is that the rich Fe-N x Active site, on the one hand, because the Fe center is positively charged, and BH4 - and 4-nitrophenol anion have negative charges, so the Fe-N x Active sites can simultaneously adsorb BH4 - ions and 4-nitrophenol anions provide the basis for the next electron transfer. The reaction mechanism is consistent with the Langmuir–Hinshelwood model. On the other hand, Fe-N x Active sites adsorb BH4 - After that, the BH bond adjacent to iron is activated, making it easier to be attacked by water molecules, accelerating the generation of ·H. At the same time, the Fe-N x The active site captures the generated ·H to form a surface Fe-H bond for attacking the nitro functional group of 4-NP. Moreover, the formation of the surface Fe-H bond effectively prevents ·H from combining with each other in the solution to generate H2, thereby improving the hydrogenation efficiency. Therefore, in the present invention, the Fe-NC single atom catalyst has a good reduction effect on 4-nitrophenol by adsorbing reaction molecules, accelerating the generation of ·H, and mediating electron transfer. Under the condition of a very small amount of Fe-NC single atom catalyst (50 mg / L), it only takes 80 seconds to react to completely reduce 20 mmol / L of 4-NP to 4-aminophenol (4-AP), and the reaction rate constant k is as high as 3.2969 min -1 , which is comparable to precious metal catalysts.
[0030] (2) In the present invention, the Fe-NC single-atom catalyst used comprises an iron atom and a three-dimensional nitrogen-doped carbon skeleton. The iron atom exists in the form of a single atom, and the iron atom coordinates with the nitrogen atom of the three-dimensional nitrogen-doped carbon skeleton to form a Fe-N x Site, Fe-N x The sites are dispersed on the three-dimensional nitrogen-doped carbon skeleton, and the total iron content is 1.1wt% to 1.8wt%. In the present invention, the three-dimensional nitrogen-doped carbon skeleton is used as the substrate, which has the advantages of stable structure and large specific surface area, so more Fe-N can be added by utilizing the coordination effect of iron and nitrogen. x The sites are stably and uniformly dispersed in the form of single atoms on the three-dimensional nitrogen-doped carbon skeleton, which makes the Fe-NC catalyst of the present invention have a larger specific surface area and richer single-atom Fe-N x sites, higher mesopore content and defect level, it is an economical hydrogenation catalyst that can be widely used with a large specific surface area, many active sites, high catalytic activity and good stability. It can be widely used to activate NaBH4, which is beneficial to the catalytic reaction.
[0031] (3) In the present invention, the preparation method of the Fe-NC single-atom catalyst is adopted, by pyrolyzing the FePc@ZIF-8 precursor, so that the ZIF-8 is pyrolyzed to generate three-dimensional nitrogen-doped carbon, and during the pyrolysis process, Fe replaces Zn to generate atomically dispersed Fe-N x The active sites are fixed on the three-dimensional nitrogen-doped carbon. At the same time, during the pyrolysis process, due to the different diffusion and migration rates of Zn and Fe, the Kirkendall effect further leads to the formation of defects and mesopores. Finally, the pyrolysis product is immersed in an acid solution and the excess metal inside the pyrolysis product is removed by pickling, which further increases the specific surface area of the product and exposes the active sites to the outside, thereby preparing a single-atom Fe-N-rich product. x The Fe-NC single atom catalyst has a large number of sites, high mesopore content and defect levels. At the same time, the preparation method of the present invention has the advantages of wide raw material sources, low cost, no need for special equipment, etc., is suitable for large-scale preparation, and is conducive to industrial production.
[0032] (4) In the present invention, the FePc@ZIF-8 precursor is prepared by the following method: according to the mass ratio of zinc salt to iron phthalocyanine of 146.9:5, zinc salt and iron phthalocyanine are dissolved in methanol to form solution A, and 2-methylimidazole is dissolved in methanol to form solution B, and then solution A is added to solution B, stirred, and the product obtained after stirring is washed and dried to obtain FePc@ZIF-8 precursor. In the present invention, Zn 2+ During the self-assembly process of ZIF-8 and 2-MI, the FePc molecules were successfully encapsulated in the ZIF-8 molecular cage by optimizing the dosage of FePc. Larger than the cavity diameter of ZIF-8 Thus, the spatial confinement effect is broken, which is beneficial to the edge zone engineering and mesopore formation. On the other hand, during the pyrolysis of ZIF-8 to generate three-dimensional nitrogen-doped carbon, Zn is evaporated due to its low boiling point (907°C), and the remaining Zn vacancies are easily replaced by Fe, which is beneficial to the generation of atomically dispersed Fe-N x Active site.
[0033] (5) In the present invention, the Fe-NC single-atom catalyst used has iron, which is cheap and readily available in nature and has low toxicity. In addition, the high catalytic efficiency of the Fe-NC single-atom catalyst makes it an excellent substitute for precious metal catalysts and is widely used in industrial production.
[0034] (6) In the present invention, the Fe-NC single-atom catalyst used has an isoelectric point of 6.5 and has a wide range of pH adaptability. It has high catalytic activity at pH 3 to 7, overcoming the shortcoming of traditional catalysts with a narrow pH adaptability range and achieving high catalytic efficiency under near-neutral conditions.
[0035] (7) In the present invention, the Fe-NC single-atom catalyst used to treat organic pollutants (such as 4-NP) shows good stability and removal rate, can be reused many times, and the removal efficiency still does not significantly decrease after being reused for 5 times, which is beneficial to reducing the treatment cost while showing good catalytic activity. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention.
[0037] Figure 1 1 is the XRD pattern of the Fe-NC single atom catalysts (FeNC-2, FeNC-5 and FeNC-10) prepared in Example 1 of the present invention.
[0038] Figure 2 TEM image of the Fe-NC single atom catalyst (FeNC-2) prepared in Example 1 of the present invention.
[0039] Figure 3 SEM and AC-HAADF-STEM images of the Fe-NC single atom catalysts (FeNC-2, FeNC-5 and FeNC-10) prepared in Example 1 of the present invention.
[0040] Figure 4This is a particle size distribution diagram of the Fe-NC single atom catalyst (FeNC-2) prepared in Example 1 of the present invention measured under a SEM electron microscope.
[0041] Figure 5 It is the adsorption-desorption isotherm diagram of the Fe-NC single atom catalyst (FeNC-2, FeNC-5 and FeNC-10) prepared in Example 1 of the present invention.
[0042] Figure 6 This is the full XPS spectrum of the Fe-NC single atom catalyst (FeNC-2) prepared in Example 1 of the present invention.
[0043] Figure 7 This is a N1s high-resolution XPS graph of the Fe-NC single-atom catalysts (FeNC-2, FeNC-5 and FeNC-10) prepared in Example 1 of the present invention.
[0044] Figure 8 This is a high-resolution XPS image of Fe 2p of the Fe-NC single-atom catalyst (FeNC-2) prepared in Example 1 of the present invention.
[0045] Fig. 9 It is the Raman spectrum of the Fe-NC single atom catalyst (FeNC-2, FeNC-5 and FeNC-10) prepared in Example 1 of the present invention.
[0046] Fig.10 This is a comparison chart of the reaction kinetic constants of different Fe-NC single atom catalysts (FeNC-2, FeNC-5 and FeNC-10) activated NaBH4 for reducing 4-NP in Example 1 of the present invention.
[0047] Fig.11 is the reaction kinetic constant (k) of the Fe-NC single atom catalyst (FeNC-2) in Example 1 of the present invention for the activation of NaBH4 for the reduction of 4-NP and the Fe-N x Linear relationship between site content (a), mesopores (b), and defects (c).
[0048] Fig.12 This is a diagram showing the cyclic catalytic effect of the Fe-NC single atom catalyst on 4-NP in Example 2 of the present invention.
[0049] Fig.13 This is a diagram showing the hydrogenation effect of the Fe-NC single atom catalyst on different pollutants in Example 3 of the present invention.
[0050] Fig.14 This is a comparison chart of the kinetic constants of the reduction reaction of 4-NP with the Fe-NC single atom catalyst and different NaBH4 dosages in Example 4 of the present invention.
[0051] Fig.15 This is a diagram showing the reduction effect of the Fe-NC single atom catalyst in Example 6 of the present invention on 4-NP in different water bodies.
[0052] Fig.16 This is a diagram showing the reduction effect of the Fe-NC single atom catalyst on 4-NP under different initial pH conditions in Example 5 of the present invention.
[0053] Fig.17 This is a Zeta potential diagram of the material surface of the Fe-NC single atom catalyst under different pH conditions in Example 5 of the present invention.
[0054] Fig.18 This is a diagram showing the reduction effect of the Fe-NC single atom catalyst in Example 6 of the present invention on 4-NP in different water bodies. DETAILED DESCRIPTION
[0055] The present invention is further described below in conjunction with the accompanying drawings and specific preferred embodiments, but the protection scope of the present invention is not limited thereby.
[0056] In the examples of the present invention, the raw materials and instruments used are all commercially available. Unless otherwise specified, the processes used are conventional processes, the equipment used are conventional equipment, and the data obtained are the average values of more than three repeated experiments.
[0057] Example 1
[0058] A method for treating organic pollutants using Fe-NC single-atom catalysts, specifically treating 4-nitrophenol (4-NP) in water using Fe-NC single-atom catalysts, comprising the following steps:
[0059] Take 5 mg of each Fe-NC single atom catalyst (FeNC-2, FeNC-5 and FeNC-10), add it to 100 mL of 0.2 mM 4-NP solution (the pH value of the solution is 5.3), stir (at a speed of 400 r / min to 600 r / min, such as 500 r / min) for 30 minutes to reach adsorption equilibrium, then add 0.1513 g of NaBH4 powder to make the NaBH4 content in the system 40 mM, and carry out reduction hydrogenation reaction for 3 minutes to complete the reduction of 4-NP.
[0060] In this embodiment, the Fe-NC single atom catalyst (FeNC-2) used includes an iron atom and a three-dimensional nitrogen-doped carbon skeleton. The iron atom exists in the form of a single atom, and the iron atom coordinates with the nitrogen atom of the three-dimensional nitrogen-doped carbon skeleton to form a Fe-N x Site, Fe-N xThe sites are dispersed on the three-dimensional nitrogen-doped carbon skeleton, where x is a positive integer ranging from 4 to 6.
[0061] In this embodiment, Fe in the Fe-NC single-atom catalyst (FeNC-2) used is mainly present in the form of positive divalent Fe, and the total iron content is 1.35 wt%.
[0062] In this embodiment, the carbon component in the three-dimensional nitrogen-doped carbon skeleton exists in the form of amorphous carbon.
[0063] In this embodiment, the nitrogen atoms in the Fe-NC single atom catalyst (FeNC-2) include, in addition to Fe-N, pyridinic nitrogen, pyrrolic nitrogen, graphitic nitrogen, and nitrogen oxide.
[0064] In this embodiment, the Fe-NC single atom catalyst (FeNC-2) presents a hollow mesoporous structure and has a prismatic dodecahedral structure.
[0065] In this embodiment, the particle size of the Fe-NC single atom catalyst (FeNC-2) is 40 nm to 120 nm.
[0066] In this embodiment, the specific surface area of the Fe-NC single atom catalyst (FeNC-2) is 879.14 m 2 / g, the pore volume at the pore diameter of 3.9nm is 0.25cm3 / g﹒nm, Fe-N x The content accounts for 38.92% of the total nitrogen content. D / I G =1.0946.
[0067] A method for preparing the Fe-NC single atom catalyst (FeNC-2) used in the present embodiment comprises the following steps:
[0068] (1) Preparation of Fe-NC precursor derived from iron phthalocyanine
[0069] 734.5 mg Zn(NO3)2·6H2O (297.49 g / mol, 2.469 mmol) and 25 mg FePc (586.37 g / mol, 0.0426 mmol) were weighed and dissolved in 50 mL methanol to form a uniform solution A. At the same time, 810.6 mg 2-methylimidazole (82.1 g / mol, 9.873 mmol) was dissolved in 50 mL methanol to form solution B. Solution A was then quickly poured into solution B and stirred in a water bath at 60 degrees for 24 hours. Finally, the obtained product was washed several times with methanol and dried overnight in a vacuum at 70°C to obtain the FePc@ZIF-8 precursor.
[0070] (2) Preparation of Fe-NC single-atom catalysts by high-temperature pyrolysis
[0071] The FePc@ZIF-8 precursor prepared above was pyrolyzed at 900°C for 3 hours under N2 atmosphere with a heating rate of 2°C / min and naturally cooled to room temperature; then, the obtained single-atom Fe-NC catalyst was immersed in 0.5M H2SO4 solution for 24 hours and washed with ultrapure water; finally, it was vacuum dried at 70°C overnight to obtain the Fe-NC single-atom catalyst, which was recorded as FeNC-2.
[0072] In this embodiment, the Fe-NC single atom catalyst (FeNC-5) used is basically the same as the Fe-NC single atom catalyst (FeNC-2), except that the total iron content in the Fe-NC single atom catalyst (FeNC-5) is 1.91wt%, the iron exists in the form of single atoms and iron atom clusters, and the specific surface area is 841.05m 2 / g, the pore volume at the pore diameter of 3.9nm is 0.126cm3 / g﹒nm, Fe-N x The content accounts for 20.20% of the total nitrogen content. D / I G =0.9666.
[0073] In this embodiment, the preparation method of the Fe-NC single atom catalyst (FeNC-5) used is basically the same as the preparation method of the Fe-NC single atom catalyst (FeNC-2), with the only difference being that the heating rate in the preparation method of the Fe-NC single atom catalyst (FeNC-5) is 5°C / min.
[0074] In this embodiment, the Fe-NC single atom catalyst (FeNC-10) used is basically the same as the Fe-NC single atom catalyst (FeNC-2), except that the total iron content in the Fe-NC single atom catalyst (FeNC-10) is 1.07 wt % and the specific surface area is 838.39 m 2 / g, the pore volume at the pore diameter of 3.9nm is 0.156cm3 / g﹒nm, and no Fe-N x site, but a new peak of pyrrolic nitrogen appeared, accounting for 12.21% of the total nitrogen content. D / I G =0.9462. In addition, iron exists in the form of single atoms and iron atom clusters.
[0075] In this embodiment, the preparation method of the Fe-NC single atom catalyst (FeNC-10) used is basically the same as the preparation method of the Fe-NC single atom catalyst (FeNC-2), with the only difference being that the heating rate in the preparation method of the Fe-NC single atom catalyst (FeNC-10) is 10°C / min.
[0076] Figure 1 The XRD patterns of Fe-NC single-atom catalysts (FeNC-2, FeNC-5 and FeNC-10) prepared in Example 1 of the present invention are shown in FIG. Figure 1 It can be seen that the XRD spectrum of the Fe-NC catalyst shows two large broad peaks at 25° and 43°, corresponding to the (002) and (101) planes of graphite carbon, respectively, and no iron oxide peaks and other impurity peaks are observed.
[0077] Figure 2 TEM image of the Fe-NC single atom catalyst (FeNC-2) prepared in Example 1 of the present invention. Figure 2 It can be seen that no lattice fringes were observed in the TEM characterization, indicating that the carbon component exists mainly in the form of amorphous phase and amorphous carbon.
[0078] Figure 3 SEM and AC-HAADF-STEM images of the Fe-NC single atom catalysts (FeNC-2, FeNC-5 and FeNC-10) prepared in Example 1 of the present invention. Figure 3 In the figure, a is the SEM image of FeNC-2, b is the AC-HAADF-STEM image of FeNC-2, c is the AC-HAADF-STEM image of FeNC-5, and d is the AC-HAADF-STEM image of FeNC-10. Figure 3 As can be seen from a, the SEM image shows that the Fe-NC single-atom catalyst (FeNC-2) retains the prismatic dodecahedral structure of ZIF-8 and has a rich mesoporous structure, which is conducive to the formation of edge host active sites. The deformation and contraction of the nanomolecular cage reflects its hollow configuration. Figure 3 b It can be seen that in the Fe-NC single-atom catalyst (FeNC-2) prepared in Example 1 of the present invention, Fe is uniformly dispersed on the Fe-NC in the form of single atoms, and the active sites are fully exposed. Figure 3 c shows that Fe in the Fe-NC single atom catalyst (FeNC-5) coexists in the form of single atoms and atomic clusters, and has good dispersion. Figure 3d shows that many bright spots are gathered on the surface of Fe-NC single atom catalyst (FeNC-10), which are identified as iron nanoparticles. The above results show that a slower heating rate is conducive to slowing down the metal aggregation of Fe and forming atomically dispersed single iron sites, thereby increasing the exposure level of active sites, making the reaction more complete, and improving the catalytic efficiency.
[0079] Figure 4 The particle size distribution diagram of the Fe-NC single atom catalyst (FeNC-2) prepared in Example 1 of the present invention measured under a SEM electron microscope. Figure 4 It can be seen that the particle size distribution range of the Fe-NC single atom catalyst is 40-120 nm, and the average geometric size is 79.82 nm, of which 90% of the particles are below 91.92 nm, 50% of the particles are below 74.68 nm, and 10% of the particles are below 51.09 nm.
[0080] Figure 5 The adsorption-desorption isotherms of the Fe-NC single-atom catalysts (FeNC-2, FeNC-5 and FeNC-10) prepared in Example 1 of the present invention are shown in FIG. Figure 5 a It can be seen that the specific surface areas of FeNC-2, FeNC-5 and FeNC-10 are 879.14 m 2 g -1 、841.05m 2 g -1 、838.39m 2 g -1 , and from Figure 5 a It can be seen that the Fe-NC single-atom catalyst conforms to type IV adsorption and has an H4 hysteresis loop, indicating that the Fe-NC single-atom catalyst contains abundant mesopores, which is consistent with Figure 5 Pore size distribution of b-5c Figure 1 To. By Figure 5 From b-5c, we can see that Figure 5 The mesopore size of b-5c is mainly concentrated in 3.40-4.30nm, and there are micropore structures below 2nm. There are mesopores and macropores distributed at 20-130nm. It is worth noting that the mesopore content is most closely related to the catalytic activity, and the mesopore content follows the order of FeNC-2>FeNC-5>FeNC-10. FeNC-2 has the best catalytic activity due to its highest mesopore content. The rich mesoporous structure is conducive to the diffusion of molecules and provides more channels for internal active sites during the reaction.
[0081] Figure 6 This is the full XPS spectrum of the Fe-NC single atom catalyst (FeNC-2) prepared in Example 1 of the present invention. Figure 6It can be seen that the Fe-NC single-atom catalyst contains four elements: Fe, N, C and O. The peak of Fe in XPS is very weak and can hardly be observed because the atomically dispersed Fe content is usually very low. In addition, the Fe content in the catalysts of FeNC-2, FeNC-5 and FeNC-10 was measured by ICP-MS to be 1.35wt%, 1.91wt% and 1.07wt% respectively.
[0082] Figure 7 This is the N1s high-resolution XPS graph of the Fe-NC single-atom catalysts (FeNC-2, FeNC-5 and FeNC-10) prepared in Example 1 of the present invention. Figure 7 It can be seen that FeNC-10 contains four types of nitrogen, including graphitic nitrogen, pyridinic nitrogen, oxidized nitrogen and pyrrolic nitrogen. As the heating rate decreases, the peak of pyrrolic nitrogen disappears, and a new peak appears between 399.2eV and 399.7eV, which is identified as MN x The results showed that FeNC-2 and FeNC-5 have rich Fe-N x Active sites. From FeNC-10 to FeNC-2, the pyridinic nitrogen content decreased from 22.79% to 13.09%, and the Fe-N x The contents increase successively, which indicates that pyridine nitrogen and Fe coordinate to form Fe-N x site, the Fe-N x The sites can not only promote the adsorption level of pollutants on the catalyst, but also serve as active components for catalytic hydrogenation, thereby obtaining more Fe-N x sites, which is more conducive to improving the adsorption and catalytic performance of the catalyst.
[0083] Figure 8 The Fe 2p high-resolution XPS image of the Fe-NC single-atom catalyst (FeNC-2) prepared in Example 1 of the present invention. Figure 8 It can be seen that in the characteristic peak of Fe, Fe 2p 1 / 2 and Fe 2p 3 / 2 The peaks of Fe-NC and Fe-N appear at around 722 eV and 709.5 eV, respectively, indicating that Fe is mainly in divalent state. x It is the main active site and can be used for hydrogen production and oxygen reduction reactions.
[0084] Fig. 9 The Raman spectra of the Fe-NC single-atom catalysts (FeNC-2, FeNC-5 and FeNC-10) prepared in Example 1 of the present invention are shown in FIG. Fig. 9 As shown, at 1339cm -1 and 1591cm -1Two peaks, D band and G band, appear at the positions of the graphene. The D band (breathing vibration mode, A1g symmetry) represents the disorder of the material, which may be caused by amorphous carbon and heteroatom doping including N and Fe. The G band (tangential mode, E2g symmetry) represents the sp 2 Hybrid graphite structure. The intensity ratio of D band to G band of FeNC-2, FeNC-5 and FeNC-10 (I D / I G ) are 1.0946, 0.9666 and 0.9462, respectively, indicating that the degree of defects and disorder increases with the decrease of heating rate. Combined with the HAADF-STEM results, it is speculated that the Fe clusters and Fe nanoparticles in FeNC-5 and FeNC-10 may reduce the exposure of amorphous carbon, resulting in the lower measured defect level.
[0085] Fig.10 This is a comparison chart of the reaction kinetic constants of different Fe-NC single atom catalysts (FeNC-2, FeNC-5 and FeNC-10) activated by NaBH4 for reducing 4-NP in Example 1 of the present invention. Fig.10 It can be seen that the reaction kinetic constants of FeNC-2, FeNC-5 and FeNC-10 are 1.60434min -1 、0.90924min -1 、0.63835min -1 , following the order of FeNC-2>FeNC-5>FeNC-10.
[0086] Fig.11 is the reaction kinetic constant (k) of the Fe-NC single atom catalyst (FeNC-2) in Example 1 of the present invention for the activation of NaBH4 for the reduction of 4-NP and the Fe-N x Linear relationship between site content (a), mesopores (b), and defects (c). Fig.11 It can be seen that the reaction kinetic constants of Fe-NC single atom catalyst for 4-NP treatment are similar to those of Fe-NC single atom catalyst. x There is a good linear correlation between site content, mesopore volume, and defect level. 2 They are 0.99958, 0.99812, and 0.97821, respectively, indicating that Fe-N x The site content is most correlated with k, followed by the mesopore volume and defect level.
[0087] Example 2
[0088] The stability of Fe-NC single atom catalyst in treating organic pollutants was investigated. Specifically, 4-NP in water was treated with Fe-NC single atom catalyst, including the following steps:
[0089] (1) 5 mg of the Fe-NC single atom catalyst (FeNC-2) prepared in Example 1 was added to 100 mL of a 0.2 mM 4-NP solution (the pH value of the solution was 5.3), and the mixture was stirred (at a speed of 400 r / min to 600 r / min, such as 500 r / min) for 30 min after ultrasonication. After reaching adsorption equilibrium, 0.1513 g of NaBH4 powder was added to make the NaBH4 content in the system 40 mM. After thorough mixing, a catalytic hydrogenation reaction was carried out for 3 min to complete the treatment of 4-NP.
[0090] (2) After the reaction in step (1) is completed, the reaction solution is filtered, and the obtained solid material (Fe-NC single atom catalyst) is washed with ultrapure water and anhydrous ethanol, and dried. The dried solid material is repeatedly treated with the 4-NP solution according to the method in step (1), and the treatment is repeated 5 times in total.
[0091] Fig.12 This is a diagram showing the cyclic catalytic effect of the Fe-NC single-atom catalyst on 4-NP in Example 2 of the present invention. Fig.12 It can be seen that after the 4-NP solution was treated with the Fe-NC single-atom catalyst for 5 cycles, the reduction rate of 4-NP within 3 minutes was still as high as 99%, and almost no decrease in catalytic efficiency was observed, which shows that the Fe-NC single-atom catalyst of the present invention has strong stability and catalytic activity. The iron ion leaching rate after the reaction was determined by ICP-MS. After 5 cycles, the Fe ion content in the system was 208.923 μg L -1 , compared with 267.124 μg L in the first cycle -1 The results show that the amount of iron ion leaching is very small. In general, the above results can prove that the catalyst has good structural stability and reusability.
[0092] Example 3
[0093] A method for treating organic pollutants using Fe-NC single-atom catalysts, specifically using Fe-NC single-atom catalysts to treat 2-nitrophenol (2-NP), 2,4-dinitrophenol (2,4-DNP), Congo red (CR), and chrome black T (EBT) in water, respectively, comprising the following steps:
[0094] Take 4 portions of the Fe-NC single atom catalyst (FeNC-2) prepared in Example 1, 5 mg each, and add them to 100 mL of 0.2 mM 2-NP and 2,4-DNP solutions, as well as 50 mg / L CR and EBT solutions, and stir ultrasonically (at a speed of 400 r / min to 600 r / min, such as 500 r / min) for 30 min. After reaching adsorption equilibrium, 0.1513 g of NaBH4 powder is added to make the NaBH4 content in the system 40 mM. After sufficient mixing, catalytic hydrogenation reaction is carried out for 3 min to complete the hydrogenation treatment of each nitrophenol and azo dye.
[0095] Fig.13 The figure is a diagram showing the hydrogenation effect of the Fe-NC single atom catalyst on different pollutants in Example 3 of the present invention. Fig.13 It can be seen that the concentrations of these pollutants (2-NP, 2,4-DNP, CR and EBT) decrease with time, and the treatment time is 90s, 10min, 8min and 50min respectively. It can be observed that with the passage of time, the corresponding pollutant peaks become weaker and weaker until they disappear, while the corresponding product peaks increase, indicating that the pollutants are completely converted into hydrogenated products. The reaction kinetic constants of hydrogenation of nitrophenol compounds follow the order of 2-NP>4-NP>2,4-DNP. This result is caused by the conjugation effect, steric hindrance effect and induction effect. Specifically, both the electron induction effect and the nitro conjugation effect can better delocalize the electron cloud on the hydroxyl group, thereby forming a more stable nitrophenol anion. Since the nitro group on 2-NP is closer to the hydroxyl group, the induction effect is stronger, making the positive charge of the nitrogen on the nitro group stronger than the positive charge on 4-NP. The results show that the negatively charged ·H is more likely to attack the nitro group on 2-NP, and the hydrogenation reaction rate is also faster. In addition, since the steric hindrance of 2,4-DNP is greater than that of mononitrophenol, the reaction activity is lower. Meanwhile, the hydrogenation reaction rate of CR is faster than that of EBT. The Fe-NC single atom catalyst in the method of the present invention has a high reduction catalytic hydrogenation efficiency for nitrophenol pollutants and azo dyes, and has wide applicability.
[0096] Example 4
[0097] A method for treating organic pollutants using Fe-NC single-atom catalysts, specifically treating 4-NP in water using Fe-NC single-atom catalysts, comprising the following steps:
[0098] Take 5 portions (5 mg) of the Fe-NC single atom catalyst (FeNC-2) prepared in Example 1 and add them to 100 mL of 0.1 mM, 0.2 mM, 0.3 mM, 0.4 mM, and 0.5 mM 4-NP solutions (pH value of the solution is 5.3), respectively, and stir ultrasonically (at a speed of 400 r / min to 600 r / min, such as 500 r / min) for 30 min. After reaching adsorption equilibrium, solid NaBH4 is added to make the NaBH4 concentration in the system 40 mM. After sufficient mixing, a catalytic reduction reaction is carried out to complete the hydrogenation reduction treatment of 4-NP under different NaBH4 concentrations.
[0099] Take 5 portions of 100 mL of a 0.2 mM 4-NP solution (the pH value of the solution is 5.3); take 5 portions of 5 mg of the Fe-NC single atom catalyst (FeNC-2) prepared in Example 1, and add them to the 0.2 mM 4-NP solution respectively, and stir ultrasonically (at a speed of 400 r / min to 600 r / min, such as 500 r / min) for 30 min. After reaching adsorption equilibrium, solid NaBH4 is added to make the NaBH4 concentration in the system 10 mM, 20 mM, 40 mM, 80 mM, and 160 mM, respectively. After fully mixing, a catalytic reduction reaction is carried out to complete the hydrogenation reduction treatment of 4-NP under different NaBH4 concentrations.
[0100] Fig.14 This is a comparison chart of the kinetic constants of the reduction reaction of 4-NP with the Fe-NC single atom catalyst and different NaBH4 dosages in Example 4 of the present invention. Fig.15 The figure is a comparison chart of the kinetic constants corresponding to the Fe-NC single atom catalyst and different 4-NP initial concentrations in Example 4 of the present invention. Fig.14 , 15 It can be seen that the kinetic constant k value is positively correlated with the NaBH4 concentration. As the 4-NP concentration increases, k first peaks at 0.20 mM and then decreases. If the reaction conforms to the Eley-Rideal mechanism, only one reactant molecule is adsorbed on the catalyst, and the reaction rate will increase with the increase of 4-NP concentration, which is inconsistent with the experimental phenomenon. The whole process conforms to the Langmuir-Hinshelwood mechanism to a large extent, indicating that the Fe-NC single atom catalyst can simultaneously adsorb BH4 - and 4-NP, and then electron transfer occurs. In this case, too low a 4-NP concentration cannot fully utilize the active sites, resulting in a low reaction rate, while too high a 4-NP concentration will squeeze out the adsorption sites of NaBH4, which is not conducive to the reaction. On the contrary, appropriately increasing the amount of NaBH4 is conducive to its contact with more adsorption sites, thereby accelerating the reaction process.
[0101] Example 5
[0102] A method for treating organic pollutants using Fe-NC single-atom catalysts, specifically treating 4-NP in water using Fe-NC single-atom catalysts, comprising the following steps:
[0103] Take 4 portions of 100 mL of 0.20 mM 4-NP solution, and adjust their pH to 3, 5, 7, and 9 respectively; take 4 portions of 5 mg of the Fe-NC single atom catalyst (FeNC-2) prepared in Example 1, and add them to the 4-NP solutions under the above different pH conditions, respectively, and stir ultrasonically (at a speed of 400 r / min to 600 r / min, such as 500 r / min) for 30 minutes. After reaching adsorption equilibrium, 0.1513 g of solid NaBH4 powder is added at the same time to make the NaBH4 content in the system 40 mM. After fully mixing, a catalytic reduction reaction is carried out to complete the reduction treatment of 4-NP under different pH conditions.
[0104] Fig.16 The figure is a diagram showing the reduction effect of the Fe-NC single atom catalyst on 4-NP under different initial pH conditions in Example 5 of the present invention. Fig.16 It can be seen that when the initial pH of 4-NP is 3, 5, 7, and 9, it takes 80s, 3min, 5min, and 7min for 0.2mM 4-NP to be completely reduced to 4-AP, and the corresponding reaction kinetic constants are 3.2969min -1 , 1.60434min -1 , 1.11428min -1 , 0.70635min -1 . This indicates that the Fe-NC single atom catalyst in the method of the present invention has a high catalytic efficiency for the hydrogenation of 4-NP at a pH of 3 to 7. Although the catalytic efficiency decreases under alkaline conditions, 4-NP can still be completely reduced within 7 minutes when the pH is 9, indicating that the Fe-NC single atom catalyst in the method of the present invention has a wide pH applicability for the reduction of 4-NP, which is conducive to practical application.
[0105] Fig.17 This is a Zeta potential diagram of the material surface of the Fe-NC single atom catalyst under different pH conditions in Example 5 of the present invention. Fig.17 The effect of pH on catalytic efficiency may be related to the trend of the surface charge of Fe-NC single-atom catalyst changing with pH value. Since the reaction conforms to the Langmuir-Hinshelwood model, the stronger the surface electrostatic adsorption, the better the catalytic effect. From the Zeta potential-pH relationship diagram ( Fig.17) It can be seen that with the increase of pH value, the electronegativity of the Fe-NC single atom catalyst surface increases. - The electrostatic repulsion between them is not conducive to the adsorption process, resulting in reduced reaction activity.
[0106] Example 6
[0107] A method for treating organic pollutants using Fe-NC single-atom catalysts, specifically treating 4-NP in water using Fe-NC single-atom catalysts, comprising the following steps:
[0108] (1) Ultrapure water, tap water, Xiangjiang River water, and Taozi Lake water were taken and impurities were filtered out using a filter membrane with a pore size of 0.45 μm, and the presence of 4-NP in the water was determined. Using these filtered waters as solvents, a 0.2 mM 4-NP solution was prepared using the standard addition method.
[0109] (2) Take 4 portions of the Fe-NC single atom catalyst (FeNC-2) prepared in Example 1, 5 mg each, and add them to the 4-NP solutions of different water bodies prepared in step (1) (the volume of these solutions is 100 mL), stir (at a speed of 400 r / min to 600 r / min, such as 500 r / min) for 30 min to reach adsorption equilibrium, and at the same time, add 0.1513 g of solid NaBH4 powder to make the NaBH4 content in the system 40 mM, thereby completing the hydrogenation treatment of 4-NP in different water samples.
[0110] Fig.18 The figure is a diagram showing the reduction effect of the Fe-NC single atom catalyst on 4-NP in different water bodies in Example 6 of the present invention. Fig.18 It can be seen that the corresponding catalytic reduction time when using the Fe-NC single-atom catalyst of the present invention to treat 4-NP in different water bodies is different, but the Fe-NC single-atom catalyst of the present invention can reduce 4-NP in various water bodies in a relatively short time, which shows that the Fe-NC single-atom catalyst prepared by the present invention has a good reduction effect on 4-NP in actual water samples, exhibits strong catalytic activity in practical applications, and can be widely used in treating nitrophenol pollutants in actual water bodies. At the same time, the catalytic reduction reaction of the Fe-NC single-atom catalyst of the present invention on 4-NP in different water bodies conforms to the first-order kinetics, and the corresponding kinetic constants in different water bodies (ultrapure water, tap water, river water and lake water) are respectively: K 超纯水 =1.5884min -1 , K 龙头水 =0.8721min -1 , K 桃子湖水 =0.7716min -1 , K湘江水 =0.7463min -1 .
[0111] Based on the above results, it can be seen that in the present invention, the Fe-NC single-atom catalyst has a good reduction effect on 4-nitrophenol by adsorbing reaction molecules, accelerating the generation of ·H, and mediating electron transfer. Under the condition of a very small amount of Fe-NC single-atom catalyst (50 mg / L), it only takes 80 seconds to reduce 20 mmol / L of 4-NP to 4-aminophenol (4-AP), and the reaction rate constant k is as high as 3.2969 min -1 , which is comparable to precious metal catalysts.
[0112] The above embodiments are only preferred implementations of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A method for treating organic pollutants using Fe-NC single-atom catalysts, characterized in that: The following steps are involved: The Fe-NC single atom catalyst is mixed with water containing organic pollutants, and NaBH4 is added for reduction and hydrogenation reaction to complete the treatment of organic pollutants in the water; the organic pollutants in the water containing organic pollutants are at least one of nitrophenol organic pollutants and dye organic pollutants; the nitrophenol organic pollutants are at least one of 2-nitrophenol, 4-nitrophenol, and 2,4-dinitrophenol; the dye organic pollutants are at least one of Congo red and chrome black T; the Fe-NC single atom catalyst includes iron atoms and a three-dimensional nitrogen-doped carbon skeleton; the iron atoms exist in the form of single atoms; the iron atoms coordinate with the nitrogen atoms of the three-dimensional nitrogen-doped carbon skeleton to form Fe-N sites; the Fe-N sites are dispersed on the three-dimensional nitrogen-doped carbon skeleton; the total iron content in the Fe-NC single atom catalyst is 1.1wt% to 1.8wt%; the Fe-NC single atom catalyst has a hollow mesoporous structure.
2. The method according to claim 1, characterized in that The initial ratio of the Fe-NC single atom catalyst to the organic pollutant is 5 mg: 0.01 mmol to 0.05 mmol; the molar ratio of NaBH4 to the organic pollutant is 1 to 16: 0.01 to 0.
05.
3. The method according to claim 2, characterized in that The initial concentration of organic pollutants in the water body containing organic pollutants is 0.1mmol / L to 0.5mmol / L; the pH of the water body containing organic pollutants is 3 to 11.
4. The method according to claim 3, characterized in that The mixing is carried out under stirring conditions, and the stirring time is 30 minutes; the rotation speed is controlled to be 400r / min to 500r / min during the reduction hydrogenation reaction; and the time of the reduction hydrogenation reaction is controlled to be 3 minutes to 25 minutes.
5. The method according to any one of claims 1 to 4, characterized in that: The total iron content in the Fe-NC single atom catalyst is 1.3 wt% to 1.5 wt%.
6. The method according to claim 5, characterized in that The total iron content in the Fe-NC single atom catalyst is 1.35 wt %.
7. The method according to claim 6, characterized in that The iron atoms in the Fe-NC single-atom catalyst are divalent; the carbon component in the three-dimensional nitrogen-doped carbon skeleton mainly exists in the form of amorphous carbon; the nitrogen atoms in the Fe-NC single-atom catalyst also exist in the form of at least one of pyridinic nitrogen, pyrrolic nitrogen, graphitic nitrogen, and nitrogen oxide; the Fe-NC single-atom catalyst has a prismatic dodecahedral structure; the particle size of the Fe-NC single-atom catalyst is 40nm to 120nm; the specific surface area of the Fe-NC single-atom catalyst is 838.39m 2 / g~879.14m 2 / g.
8. The method according to claim 7, characterized in that The Fe-NC single atom catalyst is prepared by the following method: S1. Dissolve the zinc salt and the iron phthalocyanine in methanol at a mass ratio of 146.9:5 to form a solution A; dissolve 2-methylimidazole in methanol to form a solution B; S2, adding solution A to solution B and stirring; S3, washing and drying the product obtained after stirring to obtain a FePc@ZIF-8 precursor; S4, pyrolyzing the FePc@ZIF-8 precursor; S5. Soaking the pyrolysis product in an acid solution, washing, and drying to obtain an atomically dispersed Fe-NC catalyst.
9. The method according to claim 8, characterized in that In S1, in solution A, the ratio of zinc salt to methanol is 14.69 mg: 1 mL; the zinc salt is Zn(NO3)2·6H2O; in solution B, the ratio of 2-methylimidazole to methanol is 810.6 mg: 50 mL; the molar ratio of zinc salt to 2-methylimidazole is 4: 1; In S2, the stirring is performed at a temperature of 60° C. and the stirring time is 24 h; In S3, the product is washed with methanol; the washing times are 3 times; the drying is performed under vacuum conditions; the drying temperature is 70° C.; In S4, the pyrolysis is carried out under a nitrogen atmosphere; the heating rate during the pyrolysis is 2°C min -1 ; The pyrolysis is to heat the FePc@ZIF-8 precursor to 900°C for calcination; the calcination time is 2h to 3h; In S5, the acid solution is a non-oxidizing strong acid solution; the non-oxidizing strong acid solution is a sulfuric acid solution or a hydrochloric acid solution; the concentration of the acid solution is 0.5 mM; the soaking time is 24 hours; the washing liquid used for washing is ultrapure water; the drying is carried out under vacuum conditions; and the drying temperature is 70°C.