Synthesis method of boron-doped carbon-coated graphite
The chemical vapor deposition method is used to deposit boron-doped carbon on the surface of graphite materials in lithium-ion batteries, which solves the problems of capacity loss and complicated doping process of lithium-ion batteries under fast charging conditions, and achieves optimization of electrochemical performance and environmentally friendly and efficient Production.
Patent Information
- Application Number
- CN202310181933.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-01
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-01
AI Technical Summary
The graphite anode material of existing lithium-ion batteries causes capacity loss due to lithium ion deintercalation and SEI film formation under fast charging conditions. The doping process is complex, energy-consuming, and environmentally unfriendly, making it difficult to be suitable for mass production.
The chemical vapor deposition method is used to deposit boron-doped carbon on the surface of the graphite material. The carbon-B bond is generated through the reaction of B2H6 and CO2 to form a uniform boron-doped layer, which avoids the inhomogeneity and local agglomeration of solid-phase doping and retains the graphite. Substrate properties and use recycled CO2 to reduce production costs.
It improves the charge storage and transfer rate, optimizes the electrochemical performance, enhances the lithium ion transport capability, reduces energy consumption and environmental pollution, is suitable for large-scale production, and the boron doping uniformity and cycle stability are significantly improved.
Smart Images

Figure CN116375018B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion battery preparation, and in particular to a method for synthesizing boron-doped carbon-coated graphite. Background Art
[0002] With the development of market demand for 3C digital products, power batteries and other energy storage devices, the performance of traditional lithium-ion batteries has been unable to meet the diversified needs of the market, especially in the face of the growing demand for "fast charging".
[0003] At present, the main negative electrode material of commercial lithium-ion batteries is graphite-based materials. However, the deintercalation process of lithium ions in the graphite negative electrode will strip off the graphite layer, and then continuously form a new SEI film, causing serious capacity loss. In addition, due to the structure of the graphite layer and the way of deintercalating lithium at high rates, its lithium storage performance is restricted, which also limits the development of graphite negative electrodes in the field of fast charging. Introducing heterogeneous element doping to modify graphite is one of the common means to optimize the performance of graphite negative electrode materials. Impurity elements are usually introduced by solid phase doping. For example, in patent CN201810860047.3, boron oxide, boric acid, tetraphenylboric acid, and sodium tetraphenylborate are used as boron sources. After high-speed mixing with graphite negative electrode materials, they are protectively calcined at high temperature in a nitrogen atmosphere to obtain boron-doped graphite. The modified graphite negative electrode synthesized by this method improves the graphitization degree of the graphite material and optimizes its charge and discharge capacity and high-temperature lithium storage performance. However, direct doping of graphite is difficult, requires a high temperature environment, and consumes a lot of energy. The damage to the graphite layer will affect the capacity retention rate during long cycles. In addition, the cumbersome fluorine gas modification process complicates the overall process and makes it difficult to apply it to large-scale production applications.
[0004] Patent CN201810882035.0 uses substances such as boron oxide, boric acid, tetraphenylboric acid, sodium tetraphenylborate as solid-phase boron sources, and asphalt-based soft carbon sources. After three steps of high-speed mixing, low-temperature compounding and high-temperature carbonization, boron-doped soft carbon-coated graphite is obtained. The modified graphite negative electrode synthesized by this method improves the lithium storage performance and capacity retention rate of the graphite negative electrode at high and low temperatures. However, on the one hand, due to the hygroscopicity of the boron source, it is easy to agglomerate and segregate. On the other hand, due to the large volume difference of the solid-phase mixed material, it is difficult to achieve uniformity during the actual mixing process, and the final doping uniformity is poor; and because asphalt and resin carbon sources contain a large amount of impurities, a large amount of toxic and harmful gases are inevitably generated during the high-temperature carbonization process, which is unfriendly to the environment and has high energy consumption; at the same time, impurities in the carbon source may react with boron to further reduce the doping effect, and the repeatability of the doping process is poor. In addition, the cumbersome fluorine gas modification process complicates the overall process and is difficult to apply to large-scale production applications. Summary of the invention
[0005] 1. Technical problem to be solved by the invention
[0006] In view of the above technical problems, the present invention provides a method for synthesizing boron-doped carbon-coated graphite, which is deposited on the surface of graphite material in the form of chemical vapor deposition, avoiding the inhomogeneity of solid-phase doping and the phenomenon of local agglomeration. In addition, the gas phase reaction occurs between the surface and the gap of the solid substrate, wherein the B doping occurs in the coated carbon layer, which has little effect on the substrate graphite, and retains the characteristics of the complete original graphite substrate.
[0007] 2. Technical solution
[0008] To solve the above problems, the present invention provides a technical solution: a method for synthesizing boron-doped carbon-coated graphite, comprising the following steps:
[0009] (1) placing natural graphite into a vapor deposition furnace, and evacuating the vapor deposition furnace to a vacuum;
[0010] (2) CO2 gas and B2H6 gas are introduced into the vapor deposition furnace simultaneously, and after a period of time, the gas is stopped and allowed to stand;
[0011] (3) The vapor deposition furnace is heated to a target temperature, then kept warm and cooled to room temperature. The product taken out is boron-doped carbon-coated graphite.
[0012] Optionally, the mass ratio of the natural graphite, CO2 gas and B2H6 gas is 500-100:11-33:3-11.
[0013] Optionally, the flow rate of the CO2 gas is 90-110 mL / min, the flow rate of the B2H6 gas is 40-60 mL / min, and the ventilation time of CO2 and B2H6 is 60-150 min.
[0014] Optionally, the target temperature of the vapor deposition furnace in step (3) is 500-800° C., the heating rate is 1-3° C. / min, and the insulation time is 300-400 min.
[0015] Optionally, in step (2), the concentration of CO2 gas is greater than 99%, and the concentration of B2H6 gas is greater than 99%.
[0016] Optionally, the standing time in step (2) is 90 to 150 minutes.
[0017] Optionally, the vapor deposition furnace is a CVD tube furnace.
[0018] Optionally, the method further includes step (4): condensing the mixed gas in the vapor deposition furnace and collecting the obtained CO2.
[0019] 3. Beneficial effects
[0020] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:
[0021] The synthesis method of boron-doped carbon-coated graphite proposed in the embodiment of the present application utilizes the chemical reaction of B2H6 and CO2, and is deposited on the surface of the graphite material in the form of chemical vapor deposition in a vapor deposition furnace to form a boron-doped carbon-coated graphite material. B2H6 reacts with CO2 to generate carbon, BC bonds and H2O to form boron-doped carbon, with the graphite substrate as the inner layer and the outer layer as boron-doped carbon. Boron doping changes the electronic structure state of the carbon layer, improves the charge storage and transmission rate, optimizes the electrochemical performance, and the introduction of boron doping and crystal structure defects are more conducive to the transmission of lithium ions. The gas phase coating method avoids the inhomogeneity of solid phase doping and the phenomenon of local agglomeration. And the gas phase reaction occurs between the surface and the gap of the solid substrate, and B doping occurs in the coated carbon layer, which has little effect on the substrate graphite, and retains the characteristics of the complete original graphite substrate. Using CO2 as the carbon source avoids various side reactions caused by impurities contained in the carbon source, and the reaction itself does not generate and release carbon dioxide, which is environmentally friendly. The CO2 gas used can be recycled and reused. The mixed gas in step (4) is CO2 and H2O. After removing the H2O through condensation, the CO2 can be reused, which can effectively reduce the production cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Schematic diagram of boron-doped carbon-coated graphite prepared by the synthesis method proposed in an embodiment of the present invention. DETAILED DESCRIPTION
[0023] In order to further understand the content of the present invention, the present invention is described in detail in conjunction with the accompanying drawings and embodiments.
[0024] The present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It is understood that the specific embodiments described herein are only used to explain the relevant inventions, rather than to limit the invention. It should also be noted that, for the convenience of description, only the parts related to the invention are shown in the accompanying drawings. The words "first", "second", etc. described in the present invention are set for the convenience of describing the technical solution of the present invention, and have no specific limiting effect. They are all general references and do not constitute a limiting effect on the technical solution of the present invention. It should be noted that, in the absence of conflict, the embodiments in the present application and the features in the embodiments can be combined with each other. In the description of the present invention, it should be noted that the orientation or position relationship indicated by the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inside", "outside", etc. is based on the orientation or position relationship shown in the accompanying drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention. In addition, the terms "first", "second", and "third" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance. Unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, or it can be a connection between the insides of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances. Multiple technical solutions in the same embodiment, and multiple technical solutions in different embodiments, can be arranged and combined to form new technical solutions without contradictions or conflicts, all of which are within the scope of protection required by the present invention.
[0025] A method for synthesizing boron-doped carbon-coated graphite comprises the following steps:
[0026] (1) placing natural graphite in a vapor deposition furnace and evacuating the vapor deposition furnace to a vacuum, wherein the mass of the natural graphite is 100 to 500 g;
[0027] (2) CO2 gas and B2H6 gas are introduced into the vapor deposition furnace at the same time, and the flow rate of CO2 is 90-110 mL / min; the flow rate of B2H6 is 40-60 mL / min, and the ventilation time is 60-150 min. After ventilation for 60-150 min, ventilation is stopped and allowed to stand; the mass ratio of natural graphite, CO2 gas, and B2H6 gas is 500-100:11-33:3-11.
[0028] (3) heating the vapor deposition furnace to 500-800° C. at a heating rate of 1-3° C. / min, then keeping the temperature for 300-400 min, and cooling to room temperature. The product taken out is boron-doped carbon-coated graphite;
[0029] (4) Connect the gas outlet of the vapor deposition furnace to the condenser to condense the mixed gas in the vapor deposition furnace and collect the obtained CO2.
[0030] The vapor deposition furnace is a CVD tube furnace. The chemical reaction of B2H6 and CO2 is used to deposit on the surface of the graphite material in the form of chemical vapor deposition in the vapor deposition furnace to form a boron-doped carbon-coated graphite material. B2H6 reacts with CO2 to generate carbon, BC bonds and H2O to form boron-doped carbon, with the graphite substrate as the inner layer and the outer layer as boron-doped carbon. Boron doping changes the electronic structure state of the carbon layer, improves the charge storage and transmission rate, optimizes the electrochemical performance, and the introduction of boron doping and crystal structure defects are more conducive to the transmission of lithium ions. The gas phase coating method avoids the inhomogeneity of solid phase doping and the phenomenon of local agglomeration. The gas phase reaction occurs between the surface and the gap of the solid substrate, and B doping occurs in the coated carbon layer, which has little effect on the substrate graphite, retaining the characteristics of the original graphite substrate. Using CO2 as the carbon source avoids various side reactions caused by impurities contained in the carbon source, and the reaction itself does not generate or release carbon dioxide, which is environmentally friendly. The CO2 gas used can be recycled and reused. The mixed gas in step (4) is CO2 and H2O. After removing the H2O through condensation, the CO2 can be reused, which can effectively reduce the production cost.
[0031] Example 1
[0032] (1) Place 100 g of natural graphite into a vapor deposition furnace and evacuate to vacuum;
[0033] (2) Slowly introducing CO2 and B2H6 into the vapor deposition furnace, wherein the flow rate of CO2 gas is 100 mL / min, and the flow rate of B2H6 gas is 50 mL / min; the ventilation time is 60 min, and the static time is 120 min;
[0034] (3) The vapor deposition furnace is heated to 500°C at a heating rate of 2°C / min and then kept at this temperature for 360 minutes. After the temperature is kept at this temperature, the furnace temperature is naturally cooled to room temperature, and the product in the furnace is taken out to obtain boron-doped carbon-coated graphite;
[0035] (4) The mixed gas in the vapor deposition furnace is condensed and the obtained CO2 is collected.
[0036] Example 2
[0037] (1) Place 100 g of natural graphite into a vapor deposition furnace and evacuate to vacuum;
[0038] (2) Slowly introducing CO2 and B2H6 into the vapor deposition furnace, wherein the gas flow rate of CO2 is 100 mL / min, and the gas flow rate of B2H6 is 50 mL / min; the ventilation time is 150 min, and the static time is 120 min;
[0039] (3) The vapor deposition furnace is heated to 500°C at a heating rate of 2°C / min and then kept at this temperature for 360 minutes. After the temperature is kept at this temperature, the furnace temperature is naturally cooled to room temperature, and the product in the furnace is taken out to obtain boron-doped carbon-coated graphite;
[0040] (4) The mixed gas in the vapor deposition furnace is condensed and the obtained CO2 is collected.
[0041] Example 3
[0042] (1) Place 500 g of natural graphite into a vapor deposition furnace and evacuate to vacuum;
[0043] (2) Slowly introducing CO2 and B2H6 into the vapor deposition furnace, wherein the gas flow rate of CO2 is 100 mL / min, and the gas flow rate of B2H6 is 50 mL / min; the ventilation time is 60 min, and the static time is 120 min;
[0044] (3) The vapor deposition furnace is heated to 500°C at a heating rate of 2°C / min and then kept at this temperature for 360 minutes. After the temperature is kept at this temperature, the furnace temperature is naturally cooled to room temperature, and the product in the furnace is taken out to obtain boron-doped carbon-coated graphite;
[0045] (4) The mixed gas in the vapor deposition furnace is condensed and the obtained CO2 is collected.
[0046] Example 4
[0047] (1) Place 100 g of natural graphite into a vapor deposition furnace and evacuate to vacuum;
[0048] (2) Slowly introducing CO2 and B2H6 into the vapor deposition furnace, wherein the gas flow rate of CO2 is 100 mL / min, and the gas flow rate of B2H6 is 50 mL / min; the ventilation time is 60 min, and the static time is 120 min;
[0049] (3) The vapor deposition furnace is heated to 800°C at a heating rate of 2°C / min and then kept at this temperature for 360 minutes. After the temperature is kept at this temperature, the furnace is cooled naturally to room temperature and the product in the furnace is taken out to obtain boron-doped carbon-coated graphite.
[0050] (4) The mixed gas in the vapor deposition furnace is condensed and the obtained CO2 is collected.
[0051] Comparative Example 1
[0052] Untreated natural graphite.
[0053] Comparative Example 2
[0054] Synthesize boron-doped carbon-coated graphite by simulating the method of patent CN201810893735.X:
[0055] (1) 16 g of petroleum resin (median particle size of 10 μm), 5 g of sodium tetraphenylborate (median particle size of 5 μm) and 200 g of natural graphite were placed in a beaker, 200 mL of deionized water were added, and the mixture was stirred for one hour to mix well;
[0056] (2) drying and granulating the granulated material by spray drying, placing the granulated material in a tubular carbonization furnace, heating to 1200° C. under a nitrogen atmosphere, heating for 10 hours, and naturally cooling to obtain boron-doped carbon-coated graphite;
[0057] Comparative Example 3
[0058] Synthesize boron-doped carbon-coated graphite by simulating the method of patent CN201810882035.0:
[0059] (1) 12 g of high softening point asphalt (median particle size 5 μm) and 4 g of boric acid (median particle size 8 μm) were added to 200 g of natural graphite and stirred rapidly for 1 hour in a high-speed mixer until the mixture was uniformly mixed;
[0060] (2) The mixed materials are placed in a vertical reactor, and the temperature is raised to 550° C. under a nitrogen atmosphere for 6 hours for low-temperature composite coating;
[0061] (3) The composite material is placed in a tubular carbonization furnace, heated to 1000° C. in a nitrogen atmosphere, heated for 10 hours, and naturally cooled to obtain boron-doped carbon-coated graphite.
[0062] The products prepared in Examples 1 to 4 and Comparative Examples 1 to 3 are the main active substances. The products prepared in Examples 1 to 4 and Comparative Examples 1 to 3 are used to prepare button-type lithium-ion half-cells for electrochemical performance evaluation.
[0063] The specific steps are:
[0064] (1) mixing the product, conductive agent carbon black, sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) in a mass ratio of 90:5:2:3, and using deionized water as a solvent to prepare a slurry;
[0065] (2) coating the slurry prepared in step (1) on a copper foil and baking it in a vacuum oven at 90° C. for 24 hours;
[0066] (3) Use a roller machine to roll the baked copper foil, and then use a punching machine to punch the rolled copper foil into 14 mm pole pieces;
[0067] (4) The electrode prepared in step (3) is combined with metallic lithium to form a 2025 button-type lithium-ion half-cell. The separator used is a polypropylene film (Celgard 2300), and the electrolyte is a mixed solution of 1M lithium hexafluorophosphate dissolved in equal volume ratios of ethylene carbonate and dimethyl carbonate. The entire assembly process is carried out in a glove box filled with high-purity nitrogen.
[0068] Finally, the prepared button-type lithium-ion half-cell was subjected to electrochemical testing, and the results are shown in the following table.
[0069]
[0070] After analysis, we know that:
[0071] 1. The modification effects of all embodiments are much better than those of comparative example 1, indicating that the modification of boron-doped carbon coating greatly improves the rate performance and cycle stability of graphite materials, and the lithium storage capacity is slightly improved due to the introduction of carbon coating.
[0072] 2. The modification effects of all embodiments are better than those of comparative examples 2 and 3, indicating that the uniformity of boron-doped carbon coating is improved, so that the effect of the modification method is fully exerted and the disadvantage of uneven doping in the original patent is improved.
[0073] 3. The comparison results in the examples show that: ① Extending the ventilation time and relatively increasing the amount of boron-doped carbon coating can improve the capacity performance and cycle stability, but the rate performance is not as good as that in Example 1; ② Increasing the graphite substrate and relatively reducing the amount of boron-doped carbon coating, the modification effect is lower than that in Example 1; ③ Increasing the carbonization temperature, aggravating the reaction rate, affecting the uniformity of the boron-doped carbon coating, and the modification effect is lower than that in Example 1.
[0074] In summary, in the modification of a certain graphite substrate, appropriate ventilation time and moderate reaction rate will improve the effect of boron-doped carbon coating modification. Excessive ventilation and faster reaction rate are not conducive to fully exerting the modification effect. However, the modification method proposed in the present invention improves the uniformity of boron-doped carbon coating, reduces energy consumption at a lower reaction temperature, and the pollution-free reaction process and one-step reaction modification process design are superior to other patented solutions.
[0075] The present invention and its embodiments are described schematically above, and the description is not restrictive. The drawings show only one embodiment of the present invention, and the actual structure is not limited thereto. Therefore, if a person skilled in the art is inspired by it and designs a structural method and an embodiment similar to the technical solution without creativity without departing from the purpose of the invention, they shall all fall within the protection scope of the present invention.
Claims
1. A method for synthesizing boron-doped carbon-coated graphite, characterized in that: The steps include: (1) placing natural graphite into a vapor deposition furnace, and evacuating the vapor deposition furnace to a vacuum; (2) CO2 gas and B2H6 gas are introduced into the vapor deposition furnace at the same time, and after a period of time, the gas is stopped and allowed to stand; (3) The vapor deposition furnace is heated to a target temperature, then kept warm and cooled to room temperature. The product taken out is boron-doped carbon-coated graphite.
2. The method for synthesizing boron-doped carbon-coated graphite according to claim 1, characterized in that: The mass ratio of the natural graphite, CO2 gas and B2H6 gas is 500-100:11-33:3-11.
3. The method for synthesizing boron-doped carbon-coated graphite according to claim 1, characterized in that: The flow rate of the CO2 gas is 90-110 mL / min, the flow rate of the B2H6 gas is 40-60 mL / min, and the ventilation time of CO2 and B2H6 is 60-150 min.
4. The method for synthesizing boron-doped carbon-coated graphite according to claim 1, characterized in that: The target temperature of the vapor deposition furnace in step (3) is 500-800° C., the heating rate is 1-3° C. / min, and the insulation time is 300-400 min.
5. The method for synthesizing boron-doped carbon-coated graphite according to claim 1, characterized in that: In the step (2), the concentration of CO2 gas is greater than 99%, and the concentration of B2H6 gas is greater than 99%.
6. The method for synthesizing boron-doped carbon-coated graphite according to claim 1, characterized in that: The standing time in step (2) is 90 to 150 minutes.
7. The method for synthesizing boron-doped carbon-coated graphite according to claim 1, characterized in that: The vapor deposition furnace is a CVD tube furnace.
8. The method for synthesizing boron-doped carbon-coated graphite according to claim 1, characterized in that: The method also includes step (4): condensing the mixed gas in the vapor deposition furnace and collecting the obtained CO2.
Citation Information
Cited By
A Preparation Method of Al2O3@C Composite Material
CN119059826B