Hybrid fiber reinforced phenolic aldehyde heat-proof and heat-insulating composite material and preparation method thereof

Through the hybrid reinforced phenolic resin composite material of quartz fiber, alumina fiber and zirconia fiber, combined with alternating laying and hot pressing curing technology, the anti-ablation and anti-shrinking performance problems in high temperature and high heat flow density environments are solved, and the cost is achieved Reduction and performance improvement.

CN118879019APending Publication Date: 2024-11-01SHANDONG NON METALLIC MATERIAL RESEARCH INSTITUTE
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410972224.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The prior art is difficult to take into account both the ablation and flush resistance and the high preparation cost, especially in the environment of high temperature and high heat flow density, a single quartz fiber reinforced resin-based composite material is difficult to meet the use requirements.

Method used

The hybrid reinforced phenolic resin composite material of quartz fiber, alumina fiber and zirconia fiber is used to improve the high temperature resistance, ablation and erosion resistance of the material through alternate layering structures and hot pressing and molding methods, and reduce the preparation cost.

Benefits of technology

It achieves better insulation and ablation performance under higher heat flow density environments, reduces material density and preparation costs, and improves the material's bearing and dimensioning capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879019A_ABST
    Figure CN118879019A_ABST
Patent Text Reader

Abstract

The invention relates to the field of preparation of high-performance materials, in particular to a hybrid fiber reinforced phenolic aldehyde heat prevention and insulation composite material and a preparation method thereof.The composite material comprises reinforced hybrid fibers and a phenolic resin matrix, and the reinforced hybrid fibers comprise quartz fibers and further comprise one or two of alumina fibers and zirconia fibers. The composite material can be obtained by compounding the phenolic resin matrix and the reinforced hybrid fiber to prepare a green body, hot-pressing and curing the green body, or alternatively laying and needling to prepare a prefabricated body, placing the prefabricated body in a mold, dipping the prefabricated body in a phenolic resin solution containing a curing agent, and gelatinizing and drying the prefabricated body. When the composite material is ablated at a high temperature, the phenolic resin matrix is pyrolyzed into carbon, heat can be absorbed and a carbon layer can be prevented from being oxidized under the melting and gasification effects of the quartz fibers, the aluminum oxide and zirconium oxide fibers are high in heat resistance, the structural strength can be kept, liquid layer loss and carbonization denudation are reduced, and the molten quartz, carbon, aluminum oxide and zirconium oxide fibers can be subjected to a ceramization reaction; and the ablation amount is further reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of high-value functional composite materials, and in particular to a hybrid fiber-reinforced phenolic anti-heat-insulating composite material and a preparation method thereof. Background Art

[0002] At high Mach flight speeds, the surface of near-space vehicles faces a harsh aerobic thermal environment and extremely high temperatures. Large-area ablation-resistant and heat-insulating composite materials for projectiles that are used for a long time in an aerobic thermal environment with high heat flux density and strong airflow scouring require light weight, heat insulation, ablation resistance, scouring resistance, and oxidation resistance, while also requiring low-cost materials. Phenolic resin has excellent thermal stability, flame retardancy, and high carbon residue rate due to its large aromatic ring structure and high cross-linking density, making it the most ideal matrix material for polymer-based ablation thermal protection composite materials. Carbon fiber, as a reinforcing fiber, has high thermal conductivity and poor thermal insulation effect, and its long-term ablation resistance is affected in an aerobic environment. Therefore, carbon fiber reinforced phenolic composites are not suitable for large-area external heat insulation structures of projectiles. Phenolic composites reinforced with inorganic fibers such as glass fiber, high silica fiber, quartz fiber, and basalt fiber have better thermal insulation effects than carbon fiber phenolic composites. In particular, quartz fiber has excellent comprehensive performance and is currently a commonly used reinforcing fiber for large-area external heat insulation materials in near-space.

[0003] However, when the temperature reaches 900℃, quartz fiber will crystallize and its mechanical strength will drop rapidly. When the temperature reaches 1200℃, its reinforcing effect basically disappears. When the temperature reaches 1700℃, quartz fiber melts. While absorbing heat, it will also reduce the strength of the ablated carbon layer, causing surface shedding and peeling, reducing the ablation resistance and failing to maintain the aerodynamic shape of the projectile. Ceramic fibers such as alumina fiber and zirconia fiber have excellent high temperature resistance. The continuous use temperature of alumina fiber exceeds 1200℃, and the melting temperature reaches above 2000℃. The use temperature of zirconia fiber exceeds 2000℃ and the melting temperature is 2600℃. In addition, the intrinsic thermal conductivity of ceramic fiber is low. The ablative composite material prepared as reinforcing fiber can be used in ablation environments with higher temperatures and heat flux densities. However, alumina and zirconia fibers are affected by their own structural properties, have low mechanical properties, high brittleness and low bending resistance, and low elongation at break. They are easy to break and fragment when preparing fiber preforms. In addition, their high density and high cost limit their application.

[0004] Hybrid fiber reinforced composite materials are composed of two or more fibers hybridly reinforced with a matrix. Fiber hybrid composite materials can not only maintain certain performance advantages of single fiber composite materials, but also eliminate the short board effect of mechanical, thermal and electrical properties of composite materials to a certain extent, which will greatly expand the application scope of composite materials. In terms of hybrid fiber reinforced composite materials, the main research is the hybridization of glass fiber and carbon fiber, or the hybridization of glass fiber and organic fiber, and the hybridization of organic fiber and carbon fiber. The mechanical properties of the hybrid composite materials are enhanced or toughened, and the cost can be reduced. However, there is less research on the ablation resistance of hybrid fiber reinforced resin-based composite materials. As the long-term, high-temperature and high-heat flux density working conditions faced by ablation-resistant composite materials become increasingly harsh, single quartz fiber reinforced resin-based composite materials can no longer meet the use requirements.

[0005] Chinese patent CN108440010B discloses a technical method for preparing ultra-high temperature ablation-resistant composite materials by mixing carbon fibers and metal fibers. The prepared material is used for ultra-high temperature solid engine throat liners. The material preparation process is complex and requires repeated impregnation, curing and high-temperature carbonization treatment. The material density is large and is not suitable for large-area external heat protection systems.

[0006] Chinese patent CN 111285699 B discloses a lightweight, reusable heat-insulating material, which is prepared from an erosion-resistant matrix material and an ablative phenolic composite material. The erosion-resistant matrix material is obtained by impregnating a preform composed of an upper fiber preform layer, an intermediate fiber matrix layer and a lower fiber preform layer with a ceramic matrix, and then sintering the preform, and then impregnating the ablative composite material, and gelling and curing to obtain the heat-insulating material. The fiber preform is made of one or more of quartz fiber, alumina fiber, mullite fiber, aluminum silicate fiber, high silica fiber and silicon carbide fiber. The ablative composite material has excellent ablation and heat-insulating functions, and the erosion-resistant matrix has a high bearing capacity. After use, the ablative composite material can be re-compounded to achieve reusability. However, the surface layer and the bottom layer of the material are porous ceramic-based composite materials, which are used to support the nanoporous hybrid resin-based ablative layer of the middle layer, and need to be repeatedly impregnated, sintered and cured, and the preparation process is complicated. Porous ceramic-based composite materials are brittle, have poor damage resistance, are complex to assemble, and need to be disassembled and repeatedly impregnated and alated with the composite material for repeated use, resulting in high preparation and maintenance costs.

[0007] Therefore, whether it is possible to provide a composite material with lower cost and better thermal insulation effect has become one of the focuses of the inventor's research. Summary of the invention

[0008] In view of the problems that the prior art is difficult to balance the anti-ablation and anti-scouring properties and has a high preparation cost, the present invention improves the existing quartz fiber reinforced composite material and proposes a mixed fiber reinforced phenolic thermal insulation composite material of quartz fiber, alumina fiber and zirconium oxide fiber and a preparation method thereof, so as to improve the high temperature resistance, anti-ablation and anti-scouring properties of the thermal insulation phenolic material.

[0009] The specific technical solutions of the present invention are as follows:

[0010] Firstly, a hybrid fiber reinforced phenolic heat insulation composite material is provided, comprising reinforced hybrid fibers and a phenolic resin matrix; further, the mass fraction of the reinforced hybrid fibers is 40-70%, and the mass fraction of the phenolic resin matrix is ​​30-60%;

[0011] Furthermore, the reinforcing hybrid fiber includes quartz fiber and one or two of alumina fiber and zirconia fiber; the phenolic resin matrix is ​​a mixed resin of one or more of aminophenolic resin, bariumphenolic resin, magnesiumphenolic resin, boronphenolic resin and linearphenolic resin in any proportion;

[0012] Preferably, the silica content of the quartz fiber is greater than 98%, the alumina content of the alumina fiber is greater than 80%, and the zirconium oxide content of the zirconium oxide fiber is greater than 90%.

[0013] The anti-ablation mechanism of resin-based composite materials is very complex, and a large amount of heat flow is absorbed mainly through the ablation or loss of surface materials. For quartz / phenolic composite materials, the heat absorption temperature of the composite material rises rapidly under the action of aerodynamic heat, and pyrolysis occurs after reaching the thermal decomposition temperature of phenolic resin. While absorbing a large amount of heat, pyrolysis gas is released, blocking part of the aerodynamic heating heat. The temperature continues to rise and the phenolic resin is carbonized, increasing the heat of thermal radiation and playing an effective radiation heat dissipation role. Due to the low strength of the carbonized layer, the reinforcing fiber can increase the strength of the matrix carbon. As the surface temperature reaches above 1700℃, the quartz fiber also begins to melt and absorb heat. Fused quartz has a high viscosity at high temperature. While being scour, it will also form a temporary protective layer on the ablation surface, and can react with cracked carbon to absorb heat. When the temperature is higher than 2000℃, silicon dioxide begins to evaporate and vaporize, absorbing a large amount of heat. With the evaporation of the molten product, the combustion of the residual carbon, and the continuous scouring of the high-speed airflow, the ablation material continues to consume the surface and retreat. The consumption of ablative materials includes the consumption of materials caused by thermophysical changes in materials due to aerodynamic heat and the mass loss of ablative materials caused by high-speed airflow scouring. Quartz / phenolic composite materials are suitable for medium heat flux ablative environments. When the heat flux is too high, the quartz fibers melt and gasify, the strengthening effect on the resin pyrolysis carbon layer is reduced, the mass loss of ablative materials caused by scouring increases, and the heat protection efficiency is reduced.

[0014] Therefore, the heat-insulating composite material of the present invention further comprises quartz fiber, alumina fiber and zirconia fiber mixed with reinforced phenolic resin, and finally obtains a heat-insulating composite material, which is suitable for ablation environments with higher heat flux density. The surface layer of the reinforced fiber of the heat-insulating composite material of the present invention is quartz fiber, the middle layer is quartz fiber alternately stacked with alumina fiber and zirconia fiber, and the inner layer is quartz fiber. The melting point of quartz fiber is 1720°C, and the melting points of alumina fiber and zirconia fiber reach 2000°C and 2600°C respectively. Under the pneumatic heating environment, the phenolic resin is pyrolyzed into carbon, the surface quartz fiber melts and gasifies to absorb heat, and the molten quartz can also adhere to the surface of the pyrolytic carbon layer to slow down the oxidation of the carbon layer. The middle layer is made of quartz fiber and alumina fiber or zirconia fiber and quartz fiber alternately stacked. After the surface liquid layer is washed and vaporized, quartz fiber is still continuously melted and vaporized, which plays a role in absorbing heat and anti-oxidation. Alumina and zirconia fibers can still maintain strength to reduce surface liquid layer loss and carbonized particle erosion, and reduce the ablation rate. At the same time, the molten quartz, carbon, alumina fiber, and zirconia fiber will undergo a certain ceramic reaction to reduce the amount of ablation. Since the thermal conductivity of ceramic fiber reinforced composite materials is low, the interior is still the original material layer or the resin pyrolysis layer, which cannot reach the melting temperature of quartz fiber, so the inner layer structure is still reinforced with quartz fiber.

[0015] It can be seen that the material composition provided above in this application fully utilizes the performance advantages of fiber mixing. The surface quartz fibers melt and vaporize to absorb heat. The molten quartz can also adhere to the surface of the pyrolytic carbon layer to slow down the oxidation of the carbon layer. The alumina and zirconia fibers can still maintain strength, reduce surface liquid layer loss and carbonized particle erosion. After being compounded with phenolic resin, they have better high-temperature ablation resistance and erosion resistance, and have strong load-bearing and shape-maintaining capabilities.

[0016] In addition, the present invention also provides a method for preparing the above-mentioned hybrid fiber reinforced phenolic heat-insulating composite material, and the specific steps are as follows:

[0017] 1) placing a phenolic resin in a solvent, mixing, and dissolving to obtain a phenolic resin solution;

[0018] 2) compounding the phenolic resin solution obtained in step 1) with a fiber reinforcement to obtain a fiber reinforced prepreg;

[0019] 3) Laying the fiber-reinforced prepreg obtained in step 2) to obtain a composite material blank;

[0020] 4) hot pressing and curing the composite material blank obtained in step 3) to obtain a heat-insulating composite material.

[0021] Wherein the phenolic resin in step 1) is a mixed resin of one or more of aminophenolic resin, bariumphenolic resin, magnesiumphenolic resin, boronphenolic resin and linearphenolic resin in any proportion, the solvent is one or both of ethanol and isopropanol, and the mass ratio of phenolic resin to solvent is 2:1 to 1:4;

[0022] The fiber reinforcement in step 2) is a cloth or felt with a thickness of 0.1 to 2 mm, including quartz fiber, and one or two of alumina fiber and zirconia fiber; the mass fraction of the fiber reinforcement is 40 to 70%, and the mass fraction of the phenolic resin matrix is ​​30 to 60%; during compounding, conventional methods in the field such as scraping, brushing or wet impregnation are adopted; after compounding, a fiber-reinforced prepreg can be obtained.

[0023] Step 3) The prepreg ply is divided into an outer layer, an intermediate layer and an inner layer, the outer layer is a quartz fiber reinforced prepreg ply with a thickness of 0.1 to 1 mm, the intermediate layer is a reinforced mixed fiber with a thickness of 0.5 to 10 mm, including quartz fiber, one or two of alumina fiber and zirconia fiber, which are alternately layered, and the inner layer is a quartz fiber reinforced prepreg ply with a thickness of 1 to 30 mm.

[0024] Furthermore, in step 4), the hot pressing curing molding has a curing temperature of 140 to 220° C., a molding pressure of 0.5 to 20 MPa, and a curing time of 0.5 to 8 h.

[0025] In addition, according to different material sources, the present invention also provides another method for preparing a hybrid fiber reinforced phenolic heat-insulating composite material, and the specific steps are as follows:

[0026] 1) placing a phenolic resin in a solvent containing a curing agent and mixing the phenolic resin to completely dissolve the phenolic resin to obtain a phenolic resin solution;

[0027] 2) The fiber cloth and the fiber web are alternately stacked and needle-punched to obtain a hybrid fiber three-dimensional structure needle-punched preform;

[0028] 3) placing the preform in step 2) in a mold, and pouring the phenolic resin solution in step 1) into the mold so that the preform is completely immersed in the phenolic resin solution;

[0029] 4) The mold is sealed, and the anti-heat-insulating composite material is obtained after gelation and drying.

[0030] The phenolic resin in step 1) is a mixed resin of one or more of aminophenolic resin, bariumphenolic resin, magnesiumphenolic resin, boronphenolic resin and linearphenolic resin in any proportion, the solvent includes one or both of ethanol or isopropanol, the curing agent is one or both of hexamethylenetetramine or melamine, the mass ratio of phenolic resin to solvent is 1:9 to 1:1, and the mass ratio of phenolic resin to curing agent is 19:1 to 9:1.

[0031] In step 2), the fiber-based cloth is a quartz fiber cloth, the fiber web comprises one or two of a quartz fiber web, an alumina fiber web and a zirconia fiber web, the thickness of the quartz fiber cloth is 0.1 to 2.0 mm, and the surface density of the fiber web is 30 to 200 g / m 2 ;

[0032] Furthermore, the needle-punched preform is divided into two layers, inner and outer layers, and each layer is prepared by alternating stacking; the outer layer is made of quartz fiber cloth and alumina fiber mesh or zirconia fiber mesh alternately stacked and needle-punched, the mass ratio of quartz fiber cloth to alumina fiber and / or zirconia fiber is 1:3-3:1, and the thickness is 0.5-10mm; the inner layer is made of quartz fiber base cloth and quartz fiber mesh alternately stacked and needle-punched, the thickness is 1-50mm, and the density of the final needle-punched preform is controlled by adjusting the mass ratio of quartz fiber base cloth to quartz fiber mesh; after the inner layer is alternately stacked and needle-punched, the outer layer is alternately stacked and needle-punched directly on its outer side, and the inner layer and the outer layer are continuously needle-punched to form a whole; further, the density of the needle-punched preform is 0.2-0.7g / cm 3 .

[0033] Step 3) The impregnation method includes atmospheric pressure impregnation, vacuum assisted impregnation and low pressure perfusion;

[0034] Furthermore, the atmospheric pressure impregnation is to place the needle punched preform in a mold, and impregnate the needle punched preform with the phenolic resin solution by capillary action under atmospheric pressure; the vacuum assisted impregnation is to place the needle punched preform in a sealed mold, and after the mold is evacuated, the phenolic resin solution is impregnated in the needle punched preform; the low pressure infusion is to place the needle punched preform in a sealed mold, and the phenolic resin solution is infused into the mold by low pressure to impregnate the needle punched preform. Specifically, the mass fraction of the reinforcing hybrid fiber is controlled to be 40-70%, and the mass fraction of the phenolic resin matrix is ​​controlled to be 30-60% by adjusting the concentration of the impregnation solution and the density of the needle punched preform.

[0035] Step 4) The gelation reaction temperature is 80-150°C and the time is 12-72 hours; further, the drying is to take the composite material out of the mold and dry it at a temperature of 80-120°C and normal pressure for 48-96 hours.

[0036] The hybrid fiber prepreg prepared by the above method is a low-density heat-insulating phenolic composite material, which has the characteristics of low density and good ablation resistance, and can be used in long-term working conditions of medium and low heat flux density and scouring.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] (1) The hybrid fiber reinforced phenolic resin-based heat-insulating composite material of the present invention uses quartz fiber as the main reinforcement and is mixed with alumina fiber and / or zirconia fiber, which fully utilizes the performance advantages of the mixed fibers. The surface quartz fiber undergoes melting and gasification to absorb heat, and the molten quartz can also adhere to the surface of the pyrolytic carbon layer to slow down the oxidation of the carbon layer. The alumina and zirconia fibers can still maintain strength, reduce surface liquid layer loss and carbonized particle erosion, and have better high-temperature ablation resistance and erosion resistance after being compounded with phenolic resin, and have strong load-bearing and shape-maintaining capabilities.

[0039] (2) The hybrid fiber reinforced structure used in the present invention uses alumina fiber and zirconia fiber only in the surface layer or the middle layer, and after being mixed with quartz fiber, its high temperature resistance and ablation resistance are fully utilized. After the surface quartz molten liquid layer is washed and vaporized, the mixed quartz fiber is still continuously melted and vaporized, which has a better heat absorption and anti-oxidation effect than the pure alumina or zirconia fiber layer. At the same time, the use of less alumina fiber and zirconia fiber avoids the high density and high cost of the composite material.

[0040] (3) In the inner layer of the composite material, quartz fiber is still used as a reinforcement to ensure the strength of the composite material and reduce the manufacturing cost. At the same time, the manufacturing cost of alumina fiber felt and zirconia fiber felt has been greatly reduced. The ablation resistance of the composite material has been significantly improved without increasing the manufacturing cost of the mixed fiber preform. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 3. It is a sample picture of the hybrid fiber reinforced phenolic composite material prepared in Example 1 and the quartz fiber reinforced phenolic composite material prepared in Comparative Example 1 after oxyacetylene ablation test;

[0042] Figure 2 is a SEM image of the hybrid fiber reinforced phenolic composite material prepared in Example 1 after oxyacetylene ablation experiment;

[0043] Figure 3 This is a SEM image of the quartz fiber reinforced phenolic composite material prepared in Comparative Example 1 after ablation experiment. DETAILED DESCRIPTION

[0044] The technical solution of the present invention is further described below in conjunction with specific embodiments. These embodiments are only used to illustrate the technical solution of the present invention in more detail and should not be construed as limiting the protection scope of the present invention.

[0045] Magnesium phenolic resin was selected from S157 resin of Shandong Non-metallic Materials Research Institute; type B quartz fiber cloth was purchased from Hubei Feilihua Quartz Glass Co., Ltd.; alumina fiber cloth and alumina fiber mesh were purchased from Shanghai Rongrong New Materials Technology Co., Ltd.; barium phenolic resin was purchased from Shandong Shengquan New Materials Co., Ltd.; type D quartz fiber cloth was purchased from Hubei Feilihua Quartz Glass Co., Ltd.; zirconium oxide fiber cloth was purchased from Fosman (Beijing) Technology Co., Ltd.; linear phenolic resin was purchased from Shandong Laiwu Runda New Materials Co., Ltd.; quartz fiber mesh was purchased from Hubei Feilihua Quartz Glass Co., Ltd.

[0046] The density of the composite material obtained by the present invention is tested according to the GB / T 1463-2005 test standard, and the mass ablation rate and line ablation rate of the composite material obtained by the present invention are tested according to the GJB323B-2018 test standard. The heat flux density is (4186.8±418.6) kW / m 2 The thermal conductivity of the composite material obtained by the present invention is tested according to the GB / T 10294-2008 testing standard, and the compression performance of the composite material obtained by the present invention is tested according to the GB / T 1448-2005 testing standard.

[0047] Example 1

[0048] A hybrid fiber reinforced phenolic heat-insulating composite material is composed of quartz fiber cloth, alumina fiber cloth and magnesium phenolic resin, wherein the mass fraction of reinforcing fiber is 60%, and the mass fraction of resin matrix is ​​40%. The resin is configured into a 50% ethanol solution and then impregnated with the fiber cloth, which is then layered and molded and cured to obtain the hybrid fiber reinforced phenolic composite material.

[0049] The preparation method of the above-mentioned heat-insulating composite material adopts the following steps:

[0050] Step (1): Mix magnesium phenolic resin with ethanol in a mass ratio of 1:1 to completely dissolve the resin to obtain a phenolic resin solution with a mass fraction of 50%.

[0051] Step (2): Based on a fiber mass fraction of 60% and a resin mass fraction of 40%, a phenolic solution is used to brush and impregnate a 0.2 mm thick B-type quartz fiber cloth and a 0.35 mm thick alumina fiber cloth, respectively, and the mixture is allowed to air-dry at room temperature for 48 hours to obtain a fiber-reinforced phenolic prepreg.

[0052] Step (3): Cut the prepreg into 160mm*160mm and lay them up. The inner layer is composed of 50 layers of quartz fiber reinforced prepreg with a thickness of 10mm. The middle layer is composed of 3 layers with a thickness of 1.65mm. Each layer is composed of 1 layer of alumina fiber reinforced prepreg and 1 layer of quartz fiber prepreg alternately stacked. The outer layer is composed of 2 layers of quartz fiber prepreg with a thickness of 0.4mm.

[0053] Step 3: Preheat the mold temperature to 120°C, pre-bake the laid prepreg in an oven at 100°C for 40 minutes, put it into the mold, close the mold, pressurize it with 15MPa, heat it to 180°C and keep it at this temperature for 60 minutes, then remove it from the mold after cooling it to room temperature to obtain a hybrid fiber reinforced phenolic anti-insulation composite material.

[0054] Example 2

[0055] A hybrid fiber reinforced phenolic heat-insulating composite material is composed of quartz fiber, zirconium oxide fiber and barium phenolic resin, wherein the mass fraction of the reinforcing fiber is 55%, and the mass fraction of the resin matrix is ​​45%. The prepreg is prepared and then layered, and then cured in an autoclave to obtain the hybrid fiber reinforced phenolic composite material.

[0056] The preparation method of the above-mentioned heat-insulating composite material adopts the following steps:

[0057] Step (1): Mix barium phenolic resin and ethanol in a mass ratio of 3:2, so that the resin is completely dissolved to obtain a phenolic resin solution with a mass fraction of 60%.

[0058] Step (2): according to the fiber mass fraction of 55% and the resin mass fraction of 45%, the phenolic solution is used to brush and impregnate the D-type quartz fiber cloth with a thickness of 0.3 mm and the zirconia fiber cloth with a thickness of 0.2 mm, respectively, and left to air for 78 hours to obtain a fiber-reinforced phenolic prepreg.

[0059] Step (3): Cut the prepreg into 200mm*200mm and lay them up. The inner layer is stacked with 40 layers of quartz fiber reinforced prepreg with a thickness of 12mm. The middle layer is stacked with 3 layers with a thickness of 2.1mm. Each layer is stacked alternately with 2 layers of zirconia fiber reinforced prepreg and 1 layer of quartz fiber prepreg. The outer layer is stacked with 1 layer of quartz fiber prepreg with a thickness of 0.3mm.

[0060] Step (4): Place the laid prepreg on the mold, and lay a release cloth, adhesive felt and vacuum bag on it respectively, put the prepreg with vacuum bag into an autoclave, cure it at 190°C and a pressure of 2.0 MPa for 2 hours, cool it to room temperature and remove it from the mold to obtain a mixed fiber reinforced phenolic anti-insulation composite material.

[0061] Example 3

[0062] A hybrid fiber reinforced phenolic heat-insulating composite material is composited from a hybrid fiber needle-punched preform and a linear phenolic resin, wherein a preform is prepared by stacking and needle-punching quartz fiber cloth, a quartz fiber mesh and an alumina fiber mesh, and the hybrid fiber needle-punched preform is composited with a phenolic resin solution by low-pressure infusion to obtain a hybrid fiber reinforced phenolic heat-insulating composite material.

[0063] The preparation method of the hybrid fiber reinforced phenolic heat insulation composite material adopts the following steps:

[0064] Step (1): Weigh a certain amount of linear phenolic resin and curing agent-hexamethylene amine respectively, add them into a stirring kettle containing a certain amount of isopropanol, and mechanically stir until they are completely dissolved to obtain a phenolic resin solution, wherein the mass ratio of the phenolic resin to the isopropanol is 2:3, and the mass ratio of the phenolic resin to the hexamethylene amine is 9:1.

[0065] Step (2): Mix 0.2 mm thick D-type quartz fiber cloth and 60 g / m 2 The quartz fiber mesh tire is alternately stacked and needled, and a total of 40 layers of quartz fiber cloth and quartz fiber mesh tire are laid, with a thickness of 24mm as the inner layer;

[0066] Then, the outer side of the inner layer is coated with a surface density of 80g / m 2 Alumina fiber mesh with a surface density of 60g / m 2 The quartz fiber cloth was alternately stacked and needled, with a total of 10 layers and a thickness of 6 mm to obtain a hybrid fiber needle-punched preform with a volume density of 0.48 g / cm 3 ;

[0067] Step (3): Place the preform in a mold, seal the mold, inject the phenolic resin solution into the mold, and inject the glue at a pressure of 0.4 MPa. After the hybrid fiber preform is completely impregnated, seal the mold, and perform a sol-gel reaction at 110°C for 24 hours. After taking out the sample, dry it at 100°C for 48 hours to obtain a hybrid fiber reinforced heat-insulating composite material with a density of 0.9 g / cm 3 , fiber mass fraction 54%.

[0068] Comparative Example 1

[0069] It is the same as the mixed fiber reinforced phenolic anti-insulation composite material described in Example 1, except that no alumina fiber cloth is used, and all quartz fibers are used as reinforcing fibers. The obtained composite material has poor anti-ablation performance.

[0070] Comparative Example 2

[0071] It is the same as the mixed fiber reinforced phenolic heat-insulating composite material described in Example 2, except that no zirconium oxide fiber cloth is used, and all quartz fibers are used as reinforcing fibers. The obtained composite material has poor anti-ablation performance.

[0072] Comparative Example 3

[0073] The composite material is the same as the mixed fiber reinforced phenolic heat-insulating composite material described in Example 3, except that a quartz fiber mesh is used instead of an alumina fiber mesh to prepare the needle-punched preform, and the obtained composite material has poor ablation resistance.

[0074] The inventors tested the density, linear ablation rate, mass ablation rate, thermal conductivity and compression performance of the products obtained in Examples 1 to 3 and Comparative Examples 1 to 3. The results are shown in Table 1.

[0075] Table 1 Comparison of thermal insulation material performance of Examples 1 to 3 and Comparative Examples 1 to 3

[0076]

[0077] It can be seen from Table 1 that the density, thermal conductivity and compressive strength of the composite material of Example 1 are not much different from those of Comparative Example 1, but the linear ablation rate and mass ablation rate are lower than those of Comparative Example 1. It can be seen that the anti-insulation composite material obtained in Example 1 has better ablation resistance.

[0078] The performance comparison results of Example 2 and Example 3 and Comparative Example 2 and Comparative Example 3 are similar, and the density, thermal conductivity and compressive strength are not much different, but the ablation resistance of the composite material in the examples is significantly improved.

[0079] The composite material of Example 1 and the composite material of Comparative Example 1 were subjected to oxyacetylene ablation test, the test standard was GJB 323B-2018, and the heat flux density was (4186.8±418.6) kW / m 2 . Figure 1 (a) and Figure 1 (b) are photos of the composite material of Example 1 and the composite material of Comparative Example 1 after ablation. It can be seen that in Example 1, only the surface quartz fiber layer is ablated and washed away, while the alumina fiber still maintains its original structure. The composite material has good resistance to ablation and scouring. In Comparative Example 1 after ablation, it can be seen that the multiple quartz fiber layers on the surface are ablated and washed away, and the resistance to ablation and scouring is poor.

[0080] Figure 2 This is an SEM image of the sample surface after the oxyacetylene ablation experiment of the mixed fiber-reinforced phenolic composite material in Example 1. It can be seen that there are small balls generated by the melting of quartz fibers on the surface of the alumina fibers, and there is carbon formed by the cracking of phenolic aldehyde between the alumina fibers. The alumina fibers strengthen the surface carbon layer and reduce the erosion of the carbon layer.

[0081] Figure 3 This is a SEM image of the surface of the ablated sample of Example 1. It can be seen that the surface quartz fibers are basically ablated, and some small balls are generated after cooling. There is carbon after phenolic pyrolysis on the surface, and the carbon layer is severely eroded.

[0082] In summary, compared with the quartz fiber reinforced phenolic composite material prepared by the prior art, the hybrid fiber reinforced phenolic composite material prepared in Examples 1 to 3 has no significant difference in density, compressive strength and thermal conductivity compared with Comparative Examples 1 to 3, but the mass ablation rate is slightly reduced, and the line ablation rate is significantly reduced, indicating that the hybrid fiber reinforced phenolic composite material has a reduced ablation retreat, improved anti-erosion and shape-deformation capabilities, while maintaining good mechanical properties and thermal insulation properties, and has significant performance advantages and important applications in the field of thermal insulation and ablation resistance.

[0083] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any equivalent substitutions, modifications, etc. made by technicians in this field without any creative work within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A hybrid fiber reinforced phenolic heat insulation composite material, characterized in that: The invention comprises a reinforced hybrid fiber and a phenolic resin matrix; wherein the mass fraction of the reinforced hybrid fiber is 40-70%, and the mass fraction of the phenolic resin matrix is ​​30-60%; the reinforced hybrid fiber comprises quartz fiber, and also comprises one or two of alumina fiber and zirconium oxide fiber; the phenolic resin matrix is ​​a mixed resin of one or more of aminophenolic resin, bariumphenolic resin, magnesiumphenolic resin, boronphenolic resin and linearphenolic resin in any proportion.

2. The hybrid fiber reinforced phenolic heat insulation composite material according to claim 1, characterized in that: The silica content of the quartz fiber is greater than 98%, the alumina content of the alumina fiber is greater than 80%, and the zirconium oxide content of the zirconium oxide fiber is greater than 90%.

3. The method for preparing the hybrid fiber reinforced phenolic heat-insulating composite material according to claim 1 or 2, characterized in that: The specific steps are as follows: 1) placing a phenolic resin in a solvent, mixing, and dissolving to obtain a phenolic resin solution; 2) compounding the phenolic resin solution obtained in step 1) with a fiber reinforcement to obtain a fiber reinforced prepreg; 3) Laying the fiber-reinforced prepreg obtained in step 2) to obtain a composite material blank; 4) hot pressing and curing the composite material blank obtained in step 3) to obtain a heat-insulating composite material.

4. The method for preparing the hybrid fiber reinforced phenolic heat insulation composite material according to claim 3, characterized in that: The solvent in step 1) includes one or both of ethanol and isopropanol, and the mass ratio of phenolic resin to solvent is 2:1 to 1:

4.

5. The method for preparing the hybrid fiber reinforced phenolic heat insulation composite material according to claim 3, characterized in that: In step 2), the fiber reinforcement is a cloth or felt with a thickness of 0.1 to 2 mm, including quartz fiber, and one or two of alumina fiber and zirconia fiber; the mass fraction of the fiber reinforcement is 40 to 70%, and the mass fraction of the phenolic resin matrix is ​​30 to 60%.

6. The method for preparing the hybrid fiber reinforced phenolic heat insulation composite material according to claim 3, characterized in that: Step 3) The prepreg ply is divided into an outer layer, an intermediate layer and an inner layer, the outer layer is a quartz fiber reinforced prepreg ply with a thickness of 0.1 to 1 mm; the intermediate layer is a reinforced mixed fiber with a thickness of 0.5 to 10 mm, including quartz fiber, and one or two of alumina fiber and zirconia fiber, which are alternately layered; the inner layer is a quartz fiber reinforced prepreg ply with a thickness of 1 to 30 mm.

7. The method for preparing the hybrid fiber reinforced phenolic heat insulation composite material according to claim 3, characterized in that: In step 4), the hot pressing curing molding has a curing temperature of 140 to 220° C., a molding pressure of 0.5 to 20 MPa, and a curing time of 0.5 to 8 hours.

8. The method for preparing the hybrid fiber reinforced phenolic heat insulation composite material according to claim 1 or 2, characterized in that: The specific steps are as follows: 1) placing a phenolic resin in a solvent containing a curing agent and mixing the phenolic resin to completely dissolve the phenolic resin to obtain a phenolic resin solution; 2) The fiber cloth and the fiber web are alternately stacked and needle-punched to obtain a hybrid fiber three-dimensional structure needle-punched preform; 3) placing the preform in step 2) in a mold, and pouring the phenolic resin solution in step 1) into the mold so that the preform is completely immersed in the phenolic resin solution; 4) The mold is sealed, and the anti-heat-insulating composite material is obtained after gelation and drying.

9. The method for preparing the hybrid fiber reinforced phenolic heat insulation composite material according to claim 8, characterized in that: The solvent in step 1) includes one or both of ethanol and isopropanol, the curing agent is one or both of hexamethylenetetramine and melamine, the mass ratio of phenolic resin to solvent is 1:9 to 1:1, and the mass ratio of phenolic resin to curing agent is 19:1 to 9:

1.

10. The method for preparing the hybrid fiber reinforced phenolic heat insulation composite material according to claim 8, characterized in that: In step 2), the fiber-based cloth is a quartz fiber cloth, the fiber web comprises one or two of a quartz fiber web, an alumina fiber web and a zirconia fiber web, the thickness of the quartz fiber cloth is 0.1 to 2.0 mm, and the surface density of the fiber web is 30 to 200 g / m 2 ; Step 4) The gelation reaction temperature is 80-150° C. and the time is 12-72 hours; the drying is to take the composite material out of the mold and dry it at a temperature of 80-120° C. and normal pressure for 48-96 hours.

Citation Information

Cited By

  • Composite board for subway tunnel evacuation platform and manufacturing method

    CN120137344A

  • Fireproof fiber composite board and preparation method thereof

    CN120840167A

  • Self-adaptive deformation flexible composite material and forming method and application thereof

    CN122234554A

  • Light phenolic aldehyde ablation plate and preparation method thereof

    CN122254905A