Bamboo-based micro-nano composite cellulose, preparation method and multi-scale structured cellulose film
Through DMSO/KOH/H2O three-phase solvent system and acid anhydride esterification reaction, combined with high-speed mechanical stirring, micro-nano fibrillation of cellulose is achieved, which solves the problem of difficulty in preparing cellulose micro-fibers and nano-fibers at the same time in the existing technology. The preparation process is simplified and the performance of the cellulose film is improved, enabling efficient, low-cost large-scale application.
Patent Information
- Application Number
- CN202310314116.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-03-28
AI Technical Summary
It is difficult to efficiently prepare cellulose microfibers and nanofibers simultaneously with existing technology, resulting in complex and high-cost preparation of cellulose micro-nano hybrid fiber films, and it is difficult to balance mechanical properties and smoothness requirements with existing methods.
The DMSO/KOH/H2O three-phase solvent system is used to pre-activate cellulose. Through acid anhydride esterification reaction and high-speed mechanical stirring, the micro-nano fibrillation of cellulose is achieved, simplifying the preparation process and improving the fibrillation rate. Utilize the content of bamboo. The structural differences between thick-walled and thin-walled cellulose enable one-step preparation of micron- and nano-sized cellulose hybrid materials.
It significantly simplifies the preparation process of cellulose films, reduces energy consumption, improves the toughness, haze and transparency of cellulose films, and enables high-efficiency, low-cost large-scale applications.
Smart Images

Figure CN116375891B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of natural polymer materials, and in particular to a bamboo-based micro-nano composite cellulose, a preparation method and a cellulose film with a multi-scale structure. Background Art
[0002] Plant cell walls contain an inexhaustible supply of nanomaterials: cellulose nanofibers. Natural cellulose nanofibers have excellent mechanical properties, low linear expansion coefficient, and are renewable, biodegradable, and biocompatible. As a new type of green nanomaterial, cellulose nanofibers can be widely used in packaging, composite materials, energy storage materials, coatings, and other fields. The efficient extraction and utilization of natural cellulose nanofibers meet the requirements of my country's green development and the utilization of renewable biomass resources. Among them, high-haze and high-transparency cellulose-based films are a new type of substrate material suitable for optoelectronic devices. They have the advantages of biodegradability, renewable, low price, and adjustable performance. They are expected to promote the development of optoelectronic devices in the direction of flexibility, low cost, and degradability. The performance of cellulose film is mainly affected by the structure and composition of cellulose pulp. However, the existing technology still finds it difficult to take into account the preparation efficiency, high mechanical properties (especially folding resistance), and high smoothness.
[0003] At present, nanocellulose is mainly prepared by mechanical grinding, concentrated sulfuric acid hydrolysis and TEMPO surface oxidation. Mechanical grinding does not involve the use of chemicals and does not pollute the environment, but requires repeated high-speed stirring and centrifugal separation and then high-speed stirring-separation. The preparation process takes a long time, the energy consumption is too high, and the fibrillation degree of nanocellulose is low. A more prominent disadvantage of the concentrated sulfuric acid hydrolysis method is that its yield is generally low, about 40%. The TEMPO surface oxidation method can produce cellulose nanofibers with carboxyl functional groups, but TEMPO is expensive, resulting in high cost of prepared nanocellulose. In addition, the reaction time is relatively long (generally TEMPO oxidation time is 1 to 2 hours).
[0004] Patent CN107245766A discloses a low-energy method for preparing cellulose nanofibers, which uses DMSO ionic liquid to swell the cellulose raw material, and then performs an acid anhydride esterification reaction to obtain cellulose nanofibers. However, this method can only obtain cellulose nanofibers, and the ionic liquid is expensive and the swelling time is relatively long, so it is not conducive to large-scale application.
[0005] Since cellulose nanofibers and cellulose micron fibers are obtained by different methods or processes in the prior art, one step requires the preparation of cellulose micron fibers and the other step requires the preparation of cellulose nanofibers. It is difficult to prepare micro-nano hybrid cellulose in one step. Therefore, if a cellulose micro-nano hybrid fiber film is to be prepared, at least two steps are required.
[0006] In view of this, it is necessary to provide an improved bamboo-based micro-nano composite cellulose, a preparation method and a cellulose film with a multi-scale structure to solve the above problems. Summary of the invention
[0007] The present invention aims to provide a bamboo-based micro-nano composite cellulose, a preparation method and a cellulose film with a multi-scale structure, by using a three-phase solvent system of DMSO / KOH / H 2 O can fully and evenly activate cellulose, thereby promoting the esterification reaction to increase the degree of mechanical stirring dissociation, and finally obtain micro-nano fibrillated cellulose, providing an effective way to prepare multi-scale cellulose films.
[0008] To achieve the above object, in a first aspect, the present invention provides a method for preparing nanocellulose, comprising the following steps:
[0009] (1) Prepare a mixture containing DMSO, strong base and H 2 O mixed solvent, placing the cellulose pulp in the mixed solvent for pre-activation, and then adding acid anhydride for esterification modification;
[0010] (2) subjecting the esterified slurry to high-speed mechanical stirring to obtain nanocellulose.
[0011] In this three-phase mixed solvent system, the strong base can be fully dissolved and form a stable solution, DMSO can be inserted between cellulose molecular sheets to increase the molecular gap to promote the strong base to activate the polyhydroxyl groups on the surface and inside of the cellulose, and then introduce hydrophilic and charged groups on the cellulose surface through the esterification of the acid anhydride molecules, which is conducive to weakening the intermolecular forces and generating electrostatic mutual repulsion, accelerating the dissociation of cellulose fibrils in a high-speed mechanical stirrer, and improving the degree and rate of fibrillation, and obtaining a high-yield fibrillated cellulose material. Therefore, the present invention can significantly improve the pre-activation effect only by regulating the solvent composition, thereby providing a favorable basis for efficient fibrillation.
[0012] Further, the following steps are included:
[0013] (1) 440 parts of DMSO, 2-5 parts of strong base, H 2 O 20-40 parts of a mixed solvent is prepared, and the cellulose pulp is placed in the mixed solvent for pre-activation for 5-30 minutes; 6.17-49.4 parts of anhydride are first dissolved in 110 parts of DMSO, and then added to the pre-activated cellulose pulp, washed with water and filtered to neutrality, and then redispersed in water to prepare a pulp with a mass fraction of 0.5-0.6%, and the pH is adjusted to 9.0±0.5;
[0014] (2) pouring the slurry into a high-speed mechanical stirrer at a speed of 25000-35000 RMP, crushing and stirring for 5-30 minutes to obtain nanocellulose;
[0015] Preferably, the cellulose pulp is bamboo cellulose pulp or holocellulose pulp, more preferably bamboo cellulose pulp.
[0016] Direct application of DMSO / KOH / H 2 O quasi-solvent pre-activates cellulose materials in dry and wet states (water content is about 40-50%), reducing the need for absolute drying of cellulose; the reaction conditions for cellulose defibrination are relatively mild and the preparation process takes a shorter time, so the preparation method is significantly simplified compared to the existing technology, and the energy consumption is reduced, which is convenient for large-scale application.
[0017] In a second aspect, the present invention provides a method for preparing bamboo-based micro-nano composite cellulose, comprising the following steps:
[0018] (1) Prepare a mixture containing DMSO, strong base and H 2 O mixed solvent, placing bamboo cellulose pulp in the mixed solvent for pre-activation, and then adding acid anhydride for esterification modification;
[0019] (2) The esterified slurry is subjected to high-speed mechanical stirring to obtain bamboo-based micro-nano composite cellulose.
[0020] The present invention utilizes two main structurally different components in bamboo, namely, the structural difference between thick-wall fiber cellulose and thin-wall cell cellulose in bamboo (thick-wall fiber cellulose is "difficult to dissociate" and thin-wall cell cellulose is "easy to dissociate"), and uses DMSO / KOH / H 2 O quasi-solvent activates bamboo-derived cellulose (while retaining thick-walled fiber cellulose and thin-walled cell cellulose), then introduces negatively charged carboxyl groups through surface esterification, and uses a high-speed mechanical stirrer to defibrate under the auxiliary action of electrostatic repulsion. The present invention has found that under the preparation conditions specified in the present invention, due to the difference in the degree of dissociation difficulty and the difference in the degree of reaction between thick-walled fiber cellulose and thin-walled cell cellulose, a one-step method can be achieved to obtain a cellulose micro-nano hybrid fiber material containing both micron- and nano-scale cellulose. Furthermore, micron- and nano-scale cellulose fibers can also be separated by high-speed centrifugation, so this method provides an effective way for cellulose films with multi-scale structures.
[0021] Furthermore, the mixed solvent comprises 440 parts of DMSO, 2 to 5 parts of a strong base, and 20 to 40 parts of water by mass. By adding a certain amount of water to the DMSO / KOH quasi-solvent, that is, a certain amount of water first dissolves KOH, and then a certain amount of DMSO is added to configure it into a stable suspension quasi-solvent, the consistency of subsequent activation or reaction degree is ensured. Moreover, the water-containing cellulose can be directly processed without absolute drying, with less restrictions on raw materials and higher practicality.
[0022] And / or, the strong base includes one or more of potassium hydroxide, sodium methoxide, potassium methoxide, sodium ethoxide, potassium ethoxide, sodium tert-butoxide, potassium tert-butoxide, lithium tert-butoxide, and butyl lithium, preferably potassium hydroxide. The present invention adopts a three-phase system DMSO / KOH / H 2 O, so that potassium hydroxide can be quickly dissolved in water, and then form a stable three-phase quasi-solvent system with dimethyl sulfoxide solution, making the activation reaction of potassium hydroxide on the hydroxyl group of cellulose surface more uniform.
[0023] Furthermore, the pre-activation time is 5-30 min, preferably 5-15 min, and the esterification modification time is 5-30 min, preferably 5-15 min;
[0024] And / or, the speed of the high-speed mechanical stirring is 25000-35000 RMP, and the time is 5-30 min, preferably 5-15 min. The solvent system of the present invention has better penetration effect and activation effect, so the corresponding processing time can be significantly shortened.
[0025] And / or, the acid anhydride is one or more of phthalic anhydride, glutaric anhydride, maleic anhydride, succinic anhydride, octyl succinic anhydride, preferably succinic anhydride.
[0026] Furthermore, the addition of the acid anhydride includes: first dissolving 6.17-49.4 parts of the acid anhydride in 110 parts of DMSO, then adding it to the pre-activated bamboo cellulose pulp for reaction, washing and filtering to neutrality, and then redispersing it in water to prepare a pulp with a mass fraction of 0.5-0.6%; preferably, adjusting the pH of the pulp with a mass fraction of 0.5-0.6% to 9.0±0.5. The esterified cellulose pulp is prepared into an aqueous pulp with a lower concentration, and the pH value is adjusted to alkaline, which is more conducive to mechanical stirring and separation.
[0027] Preferably, the molar ratio of the acid anhydride to the anhydrous glucose unit in the bamboo cellulose pulp is (0.5-4):1.
[0028] Furthermore, the bamboo-based micro-nano composite cellulose obtained in step (2) is configured into a suspension with a mass fraction of 0.2%, and centrifuged at 12000 rpm for 5 minutes to separate the two sizes of cellulose fibers, wherein the upper colloid is cellulose nanofibers and the lower colloid is cellulose micron fibers.
[0029] Furthermore, the solid content of the bamboo cellulose pulp is 50-100%, and the bamboo cellulose pulp contains thick-walled fibers and thin-walled cells; in this way, the difference in the organizational structure of thick-walled fibers and thin-walled cells is cleverly utilized, and under the preparation method of the present invention, the two can be further dissociated to obtain cellulose fibers of two scales; at the same time, experiments show that the mixture of cellulose fibers of the two scales can be directly used for the preparation of high-performance cellulose film, and no formula adjustment is required. Therefore, the present invention does not need to separate the components of different structures in the bamboo material, which significantly simplifies the dissociation step of the bamboo material.
[0030] Preferably, the preparation of the bamboo cellulose pulp comprises: placing bamboo in a peracetic acid solution, reacting at 75-95°C for 4-8 hours, washing with water until neutral, placing in a potassium hydroxide solution at 75-95°C, reacting for 2-4 hours, and then washing with water until neutral to obtain bamboo cellulose pulp. The bamboo material can be bamboo flakes or crushed bamboo powder material. The non-cellulose components in the bamboo material can be removed by oxidation with peracetic acid. The concentration of the peracetic acid solution is 4-10wt%; the mass ratio of bamboo to peracetic acid is 1:(8-15); the mass fraction of the potassium hydroxide solution is 2-6%.
[0031] In a third aspect, the present invention provides a bamboo-based micro-nano composite cellulose obtained by any of the preparation methods described above, wherein the mass ratio of cellulose nanofibers to cellulose micron fibers in the bamboo-based micro-nano composite cellulose is 1:5 to 10:1, preferably 8:9 to 7:1, and the carboxyl content is 0.6 to 1.7 mmol / g.
[0032] And / or, the diameter of the cellulose nanofiber is 1.5-10nm, preferably 2-4nm, and the average diameter is preferably 2-3nm; the diameter of the cellulose microfiber is 2-25μm, preferably 10-20μm, and the average diameter is preferably 13-18μm. The bamboo-based micro-nano composite cellulose of this composition is used in the preparation of cellulose film, which can significantly improve its toughness, haze and transparency.
[0033] In a fourth aspect, the present invention provides a cellulose film with a multi-scale structure, which is prepared by using the bamboo-based micro-nano composite cellulose obtained by any of the preparation methods described above, or by using the bamboo-based micro-nano composite cellulose.
[0034] Furthermore, the bamboo-based micro-nano composite cellulose is prepared into a water suspension with a concentration of 0.1-0.8wt%, and after removing bubbles by ultrasound, it is poured into a template substrate and solidified into a film; preferably, the concentration of the water suspension is 0.2-0.4wt%. The multi-scale structured cellulose film prepared by the present invention has excellent performance, and the method is simple, which is easy to promote and apply.
[0035] The beneficial effects of the present invention are as follows:
[0036] 1. The preparation method of nanocellulose provided by the present invention is configured into a stable suspension quasi-solvent by adding a certain amount of water to the DMSO / strong base quasi-solvent, thereby ensuring the consistency of subsequent activation or reaction degree. The solvent system can be used to pre-activate cellulose materials in a wet and dry state, reducing the step of absolutely drying the cellulose. By adding a certain amount of acid anhydride esterified cellulose, hydrophilic and charged groups are introduced on the surface of cellulose, which is conducive to weakening the intermolecular forces and generating electrostatic mutual repulsion, accelerating the dissociation of cellulose fibrils in a high-speed mechanical stirrer, and improving the degree and rate of fibrillation, thereby obtaining a high-yield fibrillated cellulose material.
[0037] 2. The preparation method of bamboo-based micro-nano composite cellulose provided by the present invention cleverly utilizes the structural difference between thick-wall fiber cellulose and thin-wall cell cellulose in bamboo materials, and uses DMSO / KOH / H 2 The invention can realize a one-step method to obtain a cellulose micro-nano hybrid fiber material containing both micron- and nano-scale cellulose without separating components of different structures in the bamboo material, thereby significantly simplifying the dissociation step of the bamboo material.
[0038] 3. The multi-scale structured cellulose film provided by the present invention can be directly prepared by using the bamboo-based micro-nano composite cellulose obtained by a one-step method, without the need to adjust the formula, and has good toughness, high haze and transparency. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0040] Figure 1 For DMSO / KOH / H 2O pre-activates bamboo cellulose, then uses succinic anhydride to perform surface chemical modification, and finally uses a high-speed mechanical mixer to defibrinate the obtained cellulose micro-nano fiber colloid;
[0041] Figure 2 A photo of a highly transparent and flexible cellulose film (using DMSO / KOH / H 2 O system, reaction conditions: the molar ratio of succinic anhydride to anhydroglucose units is 4:1);
[0042] Figure 3 The SEM microscopic morphology of the surface of the multi-scale structured cellulose film;
[0043] Figure 4 To obtain the AFM morphology of cellulose nanofibers with a diameter of about 2 to 3 nm (reaction conditions: the molar ratio of succinic anhydride to anhydroglucose units was 4:1);
[0044] Figure 5 This is a real picture of cellulose film (using DMSO / KOH / H 2 O system, reaction conditions: the molar ratio of succinic anhydride to anhydroglucose units is 0.5:1);
[0045] Figure 6 This is a physical picture of the cellulose film (using anhydrous DMSO / KOH system, reaction conditions: the molar ratio of succinic anhydride to anhydroglucose units is 4:1). DETAILED DESCRIPTION
[0046] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0047] Example 1
[0048] A method for preparing bamboo-based micro-nano composite cellulose and cellulose film comprises the following steps:
[0049] 1. Preparation of dry and wet bamboo cellulose pulp
[0050] 1) Put the bamboo slices into a peracetic acid solution with a concentration of 8%, the mass ratio of the bamboo slices to the peracetic acid solution is 1:10, react at 85° C. for 4 hours, then filter and wash with water until neutral.
[0051] 2) The slurry was placed in a 5% by mass potassium hydroxide solution, reacted at 85° C. for 2 hours, and then washed with water until neutral.
[0052] 3) a portion of the slurry is placed in an oven and dried until it is absolutely dry, and the other portion is placed in the environment and air-dried to obtain bamboo cellulose slurry with a solid content of 50-100%.
[0053] 2. Preparation of bamboo-based micro-nano composite cellulose
[0054] 1) Select wet bamboo pulp cellulose pulp (solid content of 50%) as raw material.
[0055] 2) Prepare dimethyl sulfoxide (DMSO) / potassium hydroxide (KOH) / water (H 2 O) Quasi-solvent, dissolve 4.0 parts of KOH in 20.0 parts of water, then add 440.0 parts of DMSO to dissolve, and shake to mix.
[0056] 2) Weigh 40.0 parts of wet bamboo cellulose (cellulose pulp with a solid content of 50%) and add it to DMSO / KOH / H 2 O quasi-solvent and pre-activated for 10 min.
[0057] 3) Weigh 49.4 parts of succinic anhydride, the molar ratio of succinic anhydride to anhydrous glucose unit is 4:1, dissolve the above-weighed succinic anhydride in 110.0 parts of DMSO solvent, then add it to the pre-activated cellulose pulp mixture in step 2 above, react for 10 minutes, wash and filter with water until neutral, redisperse the esterified cellulose in water to prepare a pulp with a mass fraction of 0.5-0.6%, and adjust the pH to 9.0.
[0058] 4) Pour the slurry from step 3 into a high-speed mechanical stirrer at a speed of 35000 RMP, crush and stir for 10 minutes to obtain a bamboo-based micro-nano composite cellulose material with a yield of 90%, a carboxyl content of 1.7 mmol / g cellulose, and a mass ratio of micro- and nanofibers of 1 / 7. Figure 1 The figure shows the actual image of the obtained cellulose micro-nano fiber colloid. Figure 4 It can be seen that in the obtained cellulose micro-nanofiber mixture, the diameter of the micron is 14.2±6.4μm (100 micron fibers were randomly selected and measured in combination with the SEM morphology image), and the diameter of the cellulose nanofiber is about 2.2±0.4nm (100 nanofibers were selected in combination with the AFM morphology image), which is comparable to the diameter of the cellulose nanofibers obtained by the prior art, or even smaller.
[0059] 3. Preparation of cellulose mixed micro-nano fiber films with multi-scale structures
[0060] The micro-nano hybrid cellulose prepared in the above steps was prepared into a water suspension with a concentration of 0.3%. The bubbles were removed by ultrasonic for 10 minutes. The micro-nano fiber suspension after the bubbles were removed was poured into a plastic plate and dried in an oven at 40°C for 48 hours to obtain a micro-nano hybrid cellulose film with high transparency (85%) and high toughness. Figure 2 As shown in the figure, it can be seen that the micro-nano hybrid cellulose film has high transparency and good bendable surface toughness. Figure 3 It can be seen that the film contains cellulose microfibers and cellulose nanofibers. The average diameter of the cellulose microfibers is about 14 μm. The two types of cellulose fibers with different diameters help improve the comprehensive performance of the cellulose film.
[0061] Example 2
[0062] A method for preparing bamboo-based micro-nano composite cellulose and cellulose film, compared with Example 1, the difference is that the molar ratio of the acid anhydride to the anhydrous glucose unit in the bamboo cellulose pulp is different, that is, 6.17 parts of succinic anhydride are dissolved in 110.0 parts of DMSO, and shaken to mix. The mass ratio of micro- and nanofibers with a carboxyl content of 0.6mmol / g is 9 / 8, the diameter of the cellulose micron fiber is about 16.9±6.0μm (100 micron fibers are randomly selected and measured in combination with the SEM morphology), and the diameter of the cellulose nanofiber is about 2.4±0.6nm (100 nanofibers are selected in combination with the AFM morphology measurement). A micro-nano hybrid cellulose film with high transparency (80%) and high haze (87%) can be obtained by the casting method, such as Figure 5 shown.
[0063] Comparative Example 1
[0064] A method for preparing bamboo-based micro-nano composite cellulose and cellulose film, compared with Example 1, the difference is that DMSO / KOH / H 2 The quasi-solvent O does not contain water, that is, 4.0 parts of KOH are added to 440.0 parts of DMSO, shaken and mixed, and the DMSO / KOH quasi-solvent is obtained; in addition, absolutely dry bamboo cellulose pulp (solid content is 100%) is selected as the raw material, so that the system does not contain any water. The mass ratio of the obtained micro- and nano-fibers is 15 / 2, the diameter of the cellulose nanofibers is about 20.6±6.3μm (100 micron fibers are randomly selected and measured in combination with the SEM morphology), and the diameter of the cellulose nanofibers is about 2.7±0.9nm (100 nanofibers are selected in combination with the AFM morphology).
[0065] Micro-nano hybrid cellulose films with high haze (97%) but relatively low transparency (60%) can be obtained by casting, e.g. Figure 6As shown. Compared with the anhydrous reaction system, Example 1 uses a quasi-solvent system containing water and wet bamboo cellulose pulp to obtain a higher proportion of nanocellulose content, smaller diameter micro- and nanofibers, and a film with higher transparency. Compared with the same reaction conditions of succinic anhydride: anhydrous glucose unit with a molar ratio of 4:1, more nanocellulose is obtained under water-containing conditions and using wet bamboo cellulose pulp as raw material, which shows that DMSO / KOH / H 2 O has better reaction efficiency. In addition, the wet bamboo cellulose pulp used as raw material in Example 1 does not require an additional drying process, further saving energy consumption for micro-nano cellulose production. Compared with Example 2, more succinic anhydride is added in Comparative Example 1 to achieve a micro-nano fiber content equivalent to that in Example 2, but its diameter is larger than that in Example 2, and its transparency is lower than that in Example 2, indicating that the three-phase solvent system of the present invention is more conducive to the preparation of high-performance films.
[0066] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing bamboo-based micro-nano composite cellulose, characterized in that: The steps include: (1) preparing a mixed solvent containing DMSO, a strong base and H2O, placing the bamboo cellulose pulp in the mixed solvent for pre-activation, and then adding anhydride for esterification modification; the mixed solvent contains 440 parts of DMSO, 2-5 parts of a strong base, and 20-40 parts of H2O by weight; the solid content of the bamboo cellulose pulp is 50-100%; (2) The esterified slurry is subjected to high-speed mechanical stirring to obtain bamboo-based micro-nano composite cellulose.
2. The method for preparing bamboo-based micro-nano composite cellulose according to claim 1, characterized in that: The strong base includes one or more of potassium hydroxide, sodium methoxide, potassium methoxide, sodium ethoxide, potassium ethoxide, sodium tert-butoxide, potassium tert-butoxide, lithium tert-butoxide, and butyl lithium.
3. The method for preparing bamboo-based micro-nano composite cellulose according to claim 1, characterized in that: The pre-activation time is 5-30 min, and the esterification modification time is 5-30 min; And / or, the speed of the high-speed mechanical stirring is 25000-35000 RMP, and the time is 5-30 min; And / or, the acid anhydride is one or more of phthalic anhydride, glutaric anhydride, maleic anhydride, succinic anhydride, and octylsuccinic anhydride.
4. The method for preparing bamboo-based micro-nano composite cellulose according to claim 3, characterized in that: The acid anhydride is succinic anhydride.
5. The method for preparing bamboo-based micro-nano composite cellulose according to claim 1, characterized in that: The adding of the acid anhydride comprises: first dissolving 6.17-49.4 parts of the acid anhydride in 110 parts of DMSO, then adding the acid anhydride into the pre-activated bamboo cellulose pulp for reaction, washing and filtering to neutrality, and then redispersing the acid anhydride in water to prepare a pulp with a mass fraction of 0.5-0.6%.
6. The method for preparing bamboo-based micro-nano composite cellulose according to claim 5, characterized in that: The pH of the slurry with a mass fraction of 0.5-0.6% is adjusted to 9.0±0.
5.
7. The method for preparing bamboo-based micro-nano composite cellulose according to claim 5, characterized in that: The molar ratio of the acid anhydride to the anhydrous glucose unit in the bamboo cellulose pulp is (0.5-4):
1.
8. The method for preparing bamboo-based micro-nano composite cellulose according to any one of claims 1 to 7, characterized in that: The bamboo cellulose pulp contains thick-wall fiber cellulose and thin-wall cell cellulose.
9. The method for preparing bamboo-based micro-nano composite cellulose according to claim 8, characterized in that: The preparation of the bamboo cellulose pulp comprises: placing bamboo in a peracetic acid solution at 75-95° C. for reaction for 4-8 hours, washing with water until neutral, placing in a KOH solution at 75-95° C. for reaction for 2-4 hours, and then washing with water until neutral to obtain the bamboo cellulose pulp.
10. A bamboo-based micro-nano composite cellulose, characterized in that: The preparation method according to any one of claims 1 to 9 is used, wherein the mass ratio of cellulose nanofibers to cellulose microfibers in the bamboo-based micro-nano composite cellulose is 8:9 to 7:1; And / or, the diameter of the cellulose nanofiber is 1.5-10 nm; the diameter of the cellulose microfiber is 2-25 μm.
11. The bamboo-based micro-nano composite cellulose according to claim 10, characterized in that: The diameter of the cellulose nanofiber is 2-4 nm; the diameter of the cellulose microfiber is 10-20 μm.
12. A cellulose film with a multi-scale structure, characterized in that: The bamboo-based micro-nano composite cellulose is obtained by the preparation method described in any one of claims 1 to 9, or the bamboo-based micro-nano composite cellulose described in claim 10 or 11.
13. The multi-scale structured cellulose film according to claim 12, characterized in that: The bamboo-based micro-nano composite cellulose is prepared into a water suspension with a concentration of 0.1-0.8 wt %, and after removing bubbles by ultrasonic, it is poured into a template substrate and solidified into a film.
14. The multi-scale structured cellulose film according to claim 13, characterized in that: The concentration of the aqueous suspension is 0.2-0.4 wt %.
Citation Information
Patent Citations
Low energy consumption cellulose nanofiber preparation method
CN107245766A
Modified cellulose preparation method
CN109395702A
Modified lacquer and preparation method thereof
CN110894401A
Preparation method of high-strength nano cellulose-nano aramid fiber composite film
CN113336984A
Cellulose nanofiber and preparation method thereof
CN113668084A