A transparent deketoxime type silicone sealant

By compounding modified silica with high and low viscosity polydimethylsiloxane, the problem of decreased transparency of transparent silicone sealant was solved, achieving high transparency and excellent mechanical properties, and accelerating the curing speed.

CN116376511BActive Publication Date: 2026-11-17ANHUI JINGKANG BUILDING MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310427090.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-20
Publication Date
2026-11-17
Estimated Expiration
2043-04-20

AI Technical Summary

Technical Problem

The transparency of transparent silicone sealants on the market is generally low, especially after long-term storage, the transparency decreases significantly. This is mainly due to the tendency of hydrophilic silica to aggregate during the curing process, which seriously affects the transparency.

Method used

Modified silica and high-viscosity, low-viscosity α,ω-dihydroxy polydimethylsiloxane were compounded together. The surface properties of silica were improved by modifying it with alkaline amino acids. In addition, the silica was improved by working with plasticizers, crosslinking agents and catalysts to enhance dispersibility and curing speed.

Benefits of technology

It improves the transparency and mechanical properties of the sealant, shortens the surface drying time, and the transparency does not decrease significantly after long-term storage. It also improves adhesion and accelerates the curing speed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention relates to the field of sealant technology, specifically to a transparent deketoxime type silicone sealant. The transparent deketoxime type silicone sealant comprises the following components in parts by weight: 80-160 parts of high-viscosity α,ω-dihydroxypolydimethylsiloxane, 20-40 parts of low-viscosity α,ω-dihydroxypolydimethylsiloxane, 5-10 parts of modified silica, 25-45 parts of plasticizer, 10-20 parts of crosslinking agent, and 0.1-0.3 parts of catalyst. The modified silica is obtained by grafting basic amino acids onto silica. Because the basic amino acids alter the surface energy of the silica, the tendency of the modified silica to aggregate before curing in the transparent deketoxime type silicone sealant is weakened, and it will not aggregate even after long-term storage, thereby improving the transparency after curing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of sealant technology, and more particularly to a transparent ketoxime-type silicone sealant. Background Art Transparent silicone sealant is a one-component, neutral-curing, high-quality sealant, characterized by its unique high transparency. Its advantages, such as high brightness, excellent thixotropy, and high elongation, have gained widespread recognition. As a type of room temperature vulcanizing silicone rubber, it exhibits excellent performance in terms of cold resistance, heat resistance, aging resistance, water resistance, and moisture resistance.

[0002] Currently, most transparent silicone sealants on the market use hydrophilic silica as a reinforcing agent and thixotropic agent, resulting in a semi-transparent appearance. Ketooxime-type transparent silicone sealants dominate the market. The particle size, specific surface area, surface properties, and dosage of silica significantly affect the performance of the vulcanized sealant. Generally, a smaller specific surface area (larger particle size) or excessive dosage results in lower transparency and slightly poorer mechanical properties in the sealant. Conversely, a larger specific surface area (smaller particle size) leads to higher transparency.

[0003] The base adhesive of silicone sealant is α,ω-dihydroxy polydimethylsiloxane, which itself has a large number of silanol groups. The surface of hydrophilic silica contains a large number of silanol groups, which can cross-link with the base adhesive during the curing process, resulting in better compatibility and helping to improve transparency. However, the transparency of transparent silicone sealants on the market is generally not high, especially after long-term storage, its transparency decreases significantly. This is mainly because the surface of hydrophilic silica contains a large number of silanol groups that tend to aggregate before curing. Especially after long-term storage, the aggregation phenomenon is aggravated, affecting the transparency after curing. Summary of the Invention

[0004] In view of this, the purpose of this invention is to provide a transparent deketoxime type silicone sealant to solve the problem that the transparency of transparent silicone sealants currently on the market is generally poor, especially after long-term storage, their transparency decreases significantly.

[0005] To achieve the above objectives, the present invention provides a transparent ketoxime-type silicone sealant, comprising the following components in parts by weight: 80-160 parts of high-viscosity α,ω-dihydroxy polydimethylsiloxane, and low-viscosity α,ω-dihydroxy... 20-40 parts of polydimethylsiloxane, 5-10 parts of modified silica, 25-45 parts of plasticizer, and 10-20 parts of crosslinking agent. 0.1-0.3 parts of catalyst; Preferably, the high-viscosity α,ω-dihydroxypolydimethylsiloxane has a viscosity of 30000 mPa·s-80000 mPa·s at 25°C; Preferably, the low-viscosity α,ω-dihydroxypolydimethylsiloxane has a viscosity of 2000 mPa·s-5000 mPa·s at 25°C; Preferably, the specific synthesis steps of the modified silica are as follows: (1) Add silica to a mixed solution of deionized water and ethanol, then add γ-(2,3-epoxypropoxy)propyltrimethoxysilane, stir at room temperature for 3-5 h, wash and dry to obtain epoxidized silica; (2) Add epoxidized silica to ethyl acetate, then add basic amino acids and 4-dimethylaminopyridine, heat to 115-120℃, stir for 7-9h, wash and dry to obtain modified silica.

[0006] Preferably, the silica has a specific surface area of ​​100-120 m². 2 / g of hydrophilic fumed silica and a specific surface area of ​​20-100m² 2 One of the precipitated silicas in g.

[0007] Preferably, the silica has a specific surface area of ​​20-50 m². 2 / g of precipitated silica.

[0008] Preferably, in the specific synthesis steps of the modified silica, the mass ratio of silica, deionized water, ethanol and γ-(2,3-epoxypropoxy)propyltrimethoxysilane in step (1) is 5-10:40-100:10-20:0.005-0.01.

[0009] Preferably, in the specific synthesis steps of the modified silica, the mass ratio of epoxidized silica, ethyl acetate, basic amino acid and 4-dimethylaminopyridine in step (2) is 5-10:50-100:0.01-0.02:0.001-0.002.

[0010] Preferably, the basic amino acid is one of arginine, lysine, and histidine.

[0011] Preferably, the plasticizer is dimethyl silicone oil with a viscosity of 100-500 mPa·s at 25°C.

[0012] Preferably, the crosslinking agent is one or more of methyl tributanone oxime silane, vinyl tributanone oxime silane, and tetrabutanone oxime silane.

[0013] Preferably, the catalyst is one of dibutyltin dilaurate, dibutyltin diacetate, and dimethyltin dinedecanoate.

[0014] Furthermore, the present invention also provides a method for preparing the above-mentioned transparent ketoxime-type silicone sealant, the specific preparation method of which is as follows: S1: Add low-viscosity α,ω-dihydroxy polydimethylsiloxane and modified silica to the reactor and stir under vacuum for 30-60 min to obtain mixture A; S2: Add high-viscosity α,ω-dihydroxy polydimethylsiloxane and plasticizer to mixture A, and stir under vacuum for 20-40 minutes to obtain mixture B; S3: Add the crosslinking agent and catalyst to mixture B, and stir under vacuum for 20-40 minutes to obtain a transparent deketoxime type silicone sealant.

[0015] The beneficial effects of this invention are: This invention utilizes basic amino acids to modify silica, thus preparing modified silica. Because the basic amino acids alter the surface energy of silica, the modified silica exhibits a reduced tendency to aggregate in transparent deketoxime silicone sealants before curing. Even after long-term storage, it does not aggregate, thereby improving the transparency after curing.

[0016] The base adhesive of this invention is a blend of high-viscosity α,ω-dihydroxy polydimethylsiloxane and low-viscosity α,ω-dihydroxy polydimethylsiloxane. The high-viscosity α,ω-dihydroxy polydimethylsiloxane helps to improve the overall mechanical properties of the sealant after curing, while the low-viscosity α,ω-dihydroxy polydimethylsiloxane has a more flexible molecular chain and is not affected by the steric hindrance of the alkaline amino acids on the surface of the modified silica. This helps to combine with the remaining hydroxyl groups on the surface of the modified silica during curing, thereby improving the dispersion of the modified silica after curing and thus improving the transparency.

[0017] In this invention, after grafting basic amino acids onto silica, the adhesion between the sealant and the substrate is improved due to the influence of the amino groups on the surface of the basic amino acids. Furthermore, the catalytic effect of the amino groups themselves increases the curing speed and shortens the surface drying time. Detailed Implementation

[0018] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments.

[0019] The sources or properties of the raw materials used in this invention are as follows: The viscosity of high-viscosity α,ω-dihydroxy polydimethylsiloxane at 25℃ is 50000 mPa·s, the viscosity of low-viscosity α,ω-dihydroxy polydimethylsiloxane at 25℃ is 3000 mPa·s, the silica is precipitated silica with a specific surface area of ​​30 m2 / g, and the viscosity of dimethyl silicone oil at 25℃ is 200 mPa·s. Example 1

[0020] S1: Add 5g of silica to a mixed solution of 40g of deionized water and 10g of ethanol, then add 0.005g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, stir at room temperature for 3h, wash and dry to obtain epoxidized silica; S2: Add 5g of epoxidized silica to 50g of ethyl acetate, then add 0.01g of lysine and 0.001g of 4-dimethylaminopyridine was heated to 115℃ and stirred for 7 hours. After washing and drying, modified silica was obtained. S3: 20g of low-viscosity α,ω-dihydroxypolydimethylsiloxane and 5g of modified silica were added to the reaction mixture. In a reactor, the mixture is stirred under vacuum for 30 minutes to obtain mixture A; S4: Add 80g of high-viscosity α,ω-dihydroxy polydimethylsiloxane and 25g of dimethyl silicone oil to mixture A, and stir under vacuum for 20min to obtain mixture B; S5: Add 10g of methyl tributanone oxime silane and 0.1g of dibutyltin dilaurate to mixture B. The mixture was stirred in a vacuum environment for 20 minutes to obtain a transparent deketoxime type silicone sealant. Example 2

[0021] S1: Add 7.5g of silica to a mixed solution of 70g of deionized water and 15g of ethanol, then add 0.007g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, stir at room temperature for 4h, wash and dry to obtain epoxidized silica; S2: Add 7.5g of epoxidized silica to 75g of ethyl acetate, then add 0.015g of lysine and 0.002 g of 4-dimethylaminopyridine was heated to 115 °C and stirred for 8 h. After washing and drying, modified silica was obtained. S3: 30 g of low-viscosity α,ω-dihydroxypolydimethylsiloxane and 7.5 g of modified silica were added to the reaction mixture. In a reactor, the mixture is stirred under vacuum for 45 minutes to obtain mixture A; S4: Add 120g of high-viscosity α,ω-dihydroxy polydimethylsiloxane and 35g of dimethyl silicone oil to mixture A, and stir under vacuum for 30 minutes to obtain mixture B; S5: Add 15g of methyl tributanone oxime silane and 0.2g of dibutyltin dilaurate to mixture B. The mixture was stirred in a vacuum environment for 30 minutes to obtain a transparent deketoxime type silicone sealant. Example 3

[0022] S1: Add 10g of silica to a mixed solution of 100g of deionized water and 20g of ethanol, then add 0.01g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, stir at room temperature for 5h, wash and dry to obtain epoxidized silica; S2: Add 10g of epoxidized silica to 100g of ethyl acetate, then add 0.02g of lysine and 0.002 g of 4-dimethylaminopyridine was heated to 120 °C and stirred for 9 h. After washing and drying, modified silica was obtained. S3: 40 g of low-viscosity α,ω-dihydroxypolydimethylsiloxane and 10 g of modified silica were added to the reaction mixture. In a reactor, the mixture is stirred under vacuum for 60 minutes to obtain mixture A; S4: Add 160g of high-viscosity α,ω-dihydroxy polydimethylsiloxane and 45g of dimethyl silicone oil to mixture A, and stir under vacuum for 40min to obtain mixture B; S5: Add 20g of methyl tributanone oxime silane and 0.3g of dibutyltin dilaurate to mixture B. The mixture was stirred under vacuum for 40 minutes to obtain a transparent deketoxime type silicone sealant.

[0023] Example 4 S1: Same as Example 2; S2: Add 7.5g of epoxidized silica to 75g of ethyl acetate, then add 0.015g of arginine and 0.002 g of 4-dimethylaminopyridine was heated to 115 °C, stirred for 8 h, washed and dried to obtain modified silica; S3: Same as Example 2; S4: Same as Example 2; S5: Same as Example 2.

[0024] Example 5 S1: Same as Example 2; S2: Add 7.5g of epoxidized silica to 75g of ethyl acetate, then add 0.015g of histidine and 0.002 g of 4-dimethylaminopyridine was heated to 115 °C, stirred for 8 h, washed and dried to obtain modified silica; S3: Same as Example 2; S4: Same as Example 2; S5: Same as Example 2.

[0025] Comparative Example 1 S1: Add 30g of low-viscosity α,ω-dihydroxypolydimethylsiloxane and 7.5g of silica to the reactor and stir under vacuum for 45min to obtain mixture A; S2: Add 120g of high-viscosity α,ω-dihydroxy polydimethylsiloxane and 35g of dimethyl silicone oil to mixture A, and stir under vacuum for 30min to obtain mixture B; S3: Add 15g of methyl tributanone oxime silane and 0.2g of dibutyltin dilaurate to mixture B. The mixture was stirred under vacuum for 30 minutes to obtain a deketoxime type silicone sealant.

[0026] Comparative Example 2 S1: Same as Example 2; S2: Same as Example 2; S3: Add 30g of high-viscosity α,ω-dihydroxypolydimethylsiloxane and 7.5g of modified silica to the reactor and stir under vacuum for 45min to obtain mixture A; S4: Add 120g of high-viscosity α,ω-dihydroxy polydimethylsiloxane and 35g of dimethyl silicone oil to mixture A, and stir under vacuum for 30 minutes to obtain mixture B; S5: Same as Example 2. Performance Testing Surface drying time: The test was conducted according to GB / T13477.5-2017 "Test Methods for Building Sealing Materials". After storing Examples 1-5 and Comparative Examples 1-2 in a cool environment for 0 days and 30 days, the adhesive strips were extruded. The time required for no sample to adhere to the fingertip was recorded by gently touching different parts of the adhesive strip. The results are shown in Table 1.

[0027] Mechanical properties: Tested according to standard GB / T13477.8—2017 "Test Methods for Building Sealing Materials". Examples 1-5 and Comparative Examples 1-2 were stored in a cool environment for 0 days and 30 days respectively, and then cured to obtain dumbbell-shaped standard specimens. Tensile tests were performed on the dumbbell-shaped standard specimens using a tensile testing machine at a speed of 6 mm / min. The tensile strength and elongation at break were obtained, and the results are shown in Table 1.

[0028] Transmittance: According to standard GB / T 2410-2008 "Determination of transmittance and haze of transparent plastics", Examples 1-5 and Comparative Examples 1-2 were stored in a cool environment for 0 days and 30 days respectively, and then cured to obtain standard test pieces. The transmittance of the standard test pieces was measured using a Saicheng WGT-S transmittance and haze meter. The results are shown in Table 1.

[0029] Tensile bond strength: The test was conducted in accordance with GB / T13477.5-2017 "Test Methods for Building Sealing Materials". Examples 1-5 and Comparative Examples 1-2 were stored in a cool environment for 0 days and 30 days, respectively, and then cured on colorless transparent float glass. The tensile bond strength was measured using a tensile testing machine at a speed of 6 mm / min. The results are shown in Table 1.

[0030] Table 1 Performance test results of Examples 1-5 and Comparative Examples 1-2 Data Analysis: As can be seen from Examples 1-5, the transparent deketoxime type silicone sealant prepared by this invention has excellent mechanical properties and a short surface drying time. Its light transmittance can reach over 89%. After storage for 30 days and then curing, its light transmittance can still be maintained below 85%, with no significant decrease. Among them, Examples 4 and 5 show a greater decrease in light transmittance. This may be because different basic amino acids endow silica with different surface energies. The change in surface energy helps the dispersion of silica during storage. As can be seen from Examples 2 and Comparative Examples 1-2, the low viscosity base adhesive and modified silica synergistically stabilize the uniform dispersion of silica during storage. Among them, the modification of silica has the greatest impact on the stability of silica during storage.

[0031] Those skilled in the art should understand that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the invention (including the claims) is limited to these examples; within the framework of the invention, the technical features of the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other variations of the different aspects of the invention as described above, which are not provided in the details for the sake of brevity.

[0032] This invention is intended to cover all such substitutions, modifications, and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this invention should be included within the scope of protection of this invention.

Claims

1. A transparent ketoxime-type silicone sealant, characterized in that, The product comprises the following components in parts by weight: 80-160 parts of high-viscosity α,ω-dihydroxypolydimethylsiloxane, 20-40 parts of low-viscosity α,ω-dihydroxypolydimethylsiloxane, 5-10 parts of modified silica, 25-45 parts of plasticizer, 10-20 parts of crosslinking agent, and 0.1-0.3 parts of catalyst; The high-viscosity α,ω-dihydroxypolydimethylsiloxane has a viscosity of 30000 mPa·s-80000 mPa·s at 25°C. The viscosity of the low-viscosity α,ω-dihydroxypolydimethylsiloxane at 25°C is 2000 mPa·s-5000 mPa·s; The specific synthesis steps of the modified silica are as follows: (1) Add silica to a mixed solution of deionized water and ethanol, then add γ-(2,3-epoxypropoxy)propyltrimethoxysilane, stir at room temperature for 3-5 h, wash and dry to obtain epoxidized silica; (2) Add epoxidized silica to ethyl acetate, then add basic amino acids and 4-dimethylaminopyridine, heat to 115-120℃, stir for 7-9h, wash and dry to obtain modified silica.

2. The transparent ketoxime-type silicone sealant according to claim 1, characterized in that, The silica has a specific surface area of ​​100-120 m². 2 / g of hydrophilic fumed silica and a specific surface area of ​​20-100m² 2 One of the precipitated silica types, with a concentration of / g.

3. The transparent ketoxime-type silicone sealant according to claim 2, characterized in that, The silica has a specific surface area of ​​20-50 m². 2 / g of precipitated silica.

4. The transparent ketoxime-type silicone sealant according to claim 1, characterized in that, In the specific synthesis steps of the modified silica, the mass ratio of silica, deionized water, ethanol and γ-(2,3-epoxypropoxy)propyltrimethoxysilane in step (1) is 5-10:40-100:10-20:0.005-0.

01.

5. The transparent ketoxime-type silicone sealant according to claim 1, characterized in that, In the specific synthesis steps of the modified silica, the mass ratio of epoxidized silica, ethyl acetate, basic amino acids and 4-dimethylaminopyridine in step (2) is 5-10:50-100:0.01-0.02:0.001-0.

002.

6. The transparent ketoxime-type silicone sealant according to claim 1, characterized in that, The basic amino acid is one of arginine, lysine, and histidine.

7. The transparent ketoxime-type silicone sealant according to claim 1, characterized in that, The plasticizer is dimethyl silicone oil with a viscosity of 100-500 mPa·s at 25°C.

8. The transparent ketoxime-type silicone sealant according to claim 1, characterized in that, The crosslinking agent is one or more of methyl tributanone oxime silane, vinyl tributanone oxime silane, and tetrabutanone oxime silane.

9. The transparent ketoxime-type silicone sealant according to claim 1, characterized in that, The catalyst is one of dibutyltin dilaurate, dibutyltin diacetate, and dimethyltin dinedecanoate.

10. A method for preparing a transparent ketoxime-type silicone sealant according to any one of claims 1-9, characterized in that, The specific preparation method is as follows: S1: Add low-viscosity α,ω-dihydroxy polydimethylsiloxane and modified silica to the reactor and stir under vacuum for 30-60 min to obtain mixture A; S2: Add high-viscosity α,ω-dihydroxy polydimethylsiloxane and plasticizer to mixture A, and stir under vacuum for 20-40 minutes to obtain mixture B; S3: Add the crosslinking agent and catalyst to mixture B, and stir under vacuum for 20-40 minutes to obtain a transparent deketoxime type silicone sealant.

Citation Information

Patent Citations

  • Surface treatment method of special nanometer calcium carbonate for polyurethane sealant

    CN105255218A