A method for preparing ordered mesoporous carbon hollow flexible fibers and its application in sodium ion batteries
The preparation of ordered mesoporous carbon hollow flexible fibers by electrospinning and template methods has solved the problem of difficulty in taking into account both the hollow structure and the ordered structure in the prior art, and achieved good charging and discharge performance and mechanical properties of sodium ion batteries.
Patent Information
- Application Number
- CN202310273014.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-03-20
AI Technical Summary
It is difficult to prepare flexible carbon hollow fibers with both hollow structures and ordered structures in the prior art, and the carbon nanofibers prepared by electrospinning process have low performance in sodium ion batteries.
By combining electrospinning process and template method, the process of preparing flexible SiO2 fibers, alkaline solvent treatment, carbonization treatment and removal of SiO2 are carried out to obtain orderly mesoporous carbon hollow flexible fibers, avoiding the use of additional pore-forming agents. Adjust the fiber pore size and diameter to ensure mechanical properties and flexibility.
It has achieved good charging and discharge cycle performance in sodium ion batteries and is suitable for large-scale applications, avoiding the problems of reduced fiber strength and uneven pore size distribution.
Smart Images

Figure CN116377620B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method of ordered mesoporous carbon hollow flexible fibers and application of the fibers in sodium ion batteries, belonging to the technical field of new energy batteries. Background Art
[0002] One-dimensional carbon nanofiber materials have been widely used in the fields of energy conversion and energy storage due to their excellent conductivity, high aspect ratio, flexibility and other unique properties. However, solid carbon nanofibers usually only undergo interfacial reactions on the surface, and the internal space cannot provide enough reaction sites, which greatly limits their performance. At present, the common solution is to prepare hollow carbon nanofibers or porous carbon nanofibers, increase their specific surface area, and increase the reactive sites. However, due to some limitations of the synthesis method, there are few reports on the preparation of flexible carbon hollow fibers with both hollow structure and ordered structure. First of all, the current synthesis of hollow carbon fibers usually adopts coaxial electrospinning technology. Compared with uniaxial spinning, coaxial spinning is more difficult and has more stringent requirements on spinning conditions; at the same time, the hollow carbon fibers produced by coaxial spinning usually have a smaller ratio of inner and outer diameters, resulting in a thicker outer wall, otherwise it will cause a decrease in fiber strength. On the other hand, the preparation of ordered mesoporous carbon materials usually requires the help of additional polymer pore-forming agents. The use of these pore-forming agents will increase the difficulty of electrospinning, and most of them can only produce smaller mesoporous structures, which is not conducive to their promotion and use.
[0003] Sodium-ion battery is a concentration difference battery. The positive and negative electrodes are composed of two different sodium ion embedding compounds. During charging, sodium ions are deintercalated from the positive electrode and embedded into the negative electrode through the electrolyte. At this time, the negative electrode is in a sodium-rich state and the positive electrode is in a sodium-poor state. At this time, the compensating charge of electrons is supplied to the positive electrode through an external circuit to balance the charges of the positive and negative electrodes.
[0004] During discharge, sodium ions are deintercalated from the negative electrode and embedded into the positive electrode through the electrolyte. The positive electrode is in a sodium-rich state and the negative electrode is in a sodium-poor state. At this time, the compensating charge of electrons is supplied to the negative electrode through an external circuit to ensure the charge balance between the positive and negative electrodes.
[0005] In terms of raw materials, sodium-ion batteries have a greater cost advantage than lithium batteries. In terms of manufacturing process, the manufacturing process of sodium-ion batteries is similar to that of lithium batteries, so the lithium battery production line can be used.
[0006] However, the carbon nanofiber materials currently prepared by electrospinning process usually do not have sodium electrical properties or have low sodium electrical properties. Summary of the invention
[0007] The purpose of the present invention is: to address the problems and defects in the current preparation of flexible carbon hollow fibers with hollow structures and ordered structures, the present invention provides a preparation method and application of ordered mesoporous carbon hollow flexible fibers, the present invention combines electrospinning technology and template method to prepare a hollow flexible carbon fiber, and the sodium ion battery assembled with the carbon fiber exhibits good charge and discharge cycle performance.
[0008] In order to solve the above technical problems, the present invention provides a method for preparing ordered mesoporous carbon hollow flexible fibers, comprising the following steps:
[0009] Step 1): preparing flexible SiO2 fibers by electrospinning process;
[0010] Step 2): Cut the SiO2 fiber obtained in step 1) into pieces and place them in an alkaline solvent, and stir and react with a silicon source, m-diphenol and formaldehyde solution to prepare a flexible SiO2@SiO2@RF fiber;
[0011] Step 3): drying the SiO2@SiO2@RF fiber obtained in step 2) and then carbonizing it to obtain a flexible SiO2@SiO2@C fiber;
[0012] Step 4): The SiO2@SiO2@C fibers obtained in step 3) are treated with alkaline solution to remove SiO2, and then washed and freeze-dried to obtain ordered mesoporous carbon hollow flexible fibers.
[0013] Preferably, the step 1) specifically comprises: preparing an electrospinning precursor solution containing a silicon source precursor and a high molecular polymer, electrospinning the precursor solution to obtain precursor fibers, and calcining the precursor fibers to obtain flexible SiO2 fibers.
[0014] Preferably, the electrospinning precursor solution is formed by mixing a silicon source precursor solution and a high molecular polymer solution, and the silicon source precursor solution is prepared from a silicon source, an acid and a solvent.
[0015] Preferably, the silicon source is selected from at least one of tetramethyl orthosilicate, tetraethyl orthosilicate, tetrapropyl orthosilicate and tetrabutyl orthosilicate, and the acid is selected from at least one of phosphoric acid, formic acid and acetic acid.
[0016] Preferably, the alkaline solvent in step 2) is composed of ethanol, water and aqueous ammonia; and the silicon source is selected from at least one of tetramethyl orthosilicate, tetraethyl orthosilicate, tetrapropyl orthosilicate and tetrabutyl orthosilicate.
[0017] Preferably, the molar ratio of the silicon source, resorcinol and formaldehyde in step 2) is 4-6:1:1-2.
[0018] Preferably, the drying conditions in step 3) are: vacuum drying at 50-70°C for 10-15h; the carbonization treatment conditions are: heating to 600-1000°C at a heating rate of 1-3°C / min for carbonization treatment for 1-3 hours.
[0019] Preferably, the conditions for the alkali solution treatment in step 4) are: temperature 40-100° C., time 10-15 h.
[0020] The present invention also provides the ordered mesoporous carbon hollow flexible fibers prepared by the preparation method of the ordered mesoporous carbon hollow flexible fibers.
[0021] The present invention also provides the use of the ordered mesoporous carbon hollow flexible fibers prepared by the preparation method of the ordered mesoporous carbon hollow flexible fibers in sodium ion batteries.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] (1) The method for preparing an ordered mesoporous carbon hollow flexible fiber of the present invention can effectively adjust the pore size and distribution, avoiding the use of additional pore-forming agents; can effectively adjust the inner and outer diameters of the fiber to ensure a high aspect ratio;
[0024] (2) The method for preparing an ordered mesoporous carbon hollow flexible fiber of the present invention can ensure its mechanical properties and flexibility on the basis of adjusting the fiber diameter and pore size distribution, and is convenient for assembling into devices for large-scale application;
[0025] (3) The sodium ion battery assembled with the ordered mesoporous carbon hollow flexible fibers prepared by the present invention exhibits good charge and discharge cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a SEM image of the ordered mesoporous carbon hollow flexible fiber prepared in Example 1 of the present invention;
[0027] Figure 2 This is a physical picture of the ordered mesoporous carbon hollow flexible fiber prepared in Example 1 of the present invention;
[0028] Figure 3 This is a charge and discharge cycle performance test curve of the sodium ion battery assembled in Example 2 of the present invention. DETAILED DESCRIPTION
[0029] In order to make the present invention more clearly understood, preferred embodiments are described in detail below with reference to the accompanying drawings.
[0030] Example 1
[0031] A method for preparing ordered mesoporous carbon hollow flexible fibers, the specific preparation steps are as follows:
[0032] (1) First, a flexible SiO2 fiber was prepared as a template: a 10% aqueous solution of polyvinyl alcohol 1788 and a mixed solution of tetraethyl orthosilicate, phosphoric acid and water (the mass ratio of the three was 1:1:0.01) were prepared respectively; then the two were mixed in a mass ratio of 1:1, the positive electrode high voltage was 10 kV, the negative electrode high voltage was 2 kV, the syringe propulsion speed was 0.05 mm / min, and the distance between the syringe and the receiver roller was 15 cm for electrospinning; then the collected fiber precursor was transferred to a muffle furnace for calcination in air at a calcination temperature of 600 °C, a heating rate of 2 °C / min, and a time of 2 hours to obtain a flexible SiO2 fiber;
[0033] (2) Cut the obtained SiO2 fiber into small pieces and soak them in a mixed solution of 70 mL ethanol, 10 mL water and 5 mL ammonia water; add 2 mL of tetraethyl orthosilicate and 1 mL of tetrapropoxysilane to the mixed solution in sequence; then add 0.4 g of diphenylphenol and 0.56 mL of 37 wt% formaldehyde solution; continue stirring for 12 hours to prepare flexible SiO2@SiO2@RF (RF: diphenylphenol-formaldehyde) fiber;
[0034] (3) The flexible SiO2@SiO2@RF fiber was taken out, washed with ethanol, and then transferred to a vacuum drying oven for drying at 60°C for 12 hours; then transferred to a tubular furnace under nitrogen protection, heated to 800°C at a heating rate of 2°C / min for carbonization for 2 hours to obtain a flexible SiO2@SiO2@C fiber;
[0035] (4) The flexible SiO2@SiO2@C fibers were transferred to a 2M sodium hydroxide solution and heated for 12 hours to remove SiO2, and then taken out and freeze-dried for 12 hours to obtain ordered mesoporous carbon hollow flexible fibers. The fibers have good flexibility and a high aspect ratio. The electron microscope scanning results and actual photos are shown in FIG. Figures 1-2 As shown by Figure 1 It can be seen that the obtained fiber is a hollow structure with ordered mesopores. Figure 2 It can be seen that the obtained fiber has good flexibility and high fiber strength, and it rebounds after bending without breaking.
[0036] Example 2
[0037] Performance test and cycle charge and discharge performance test of sodium ion battery:
[0038] A CR 2032 button cell was assembled using a 14 mm diameter sodium metal sheet as the counter electrode, the ordered mesoporous carbon hollow flexible fiber prepared in Example 1 as the working electrode, glass fiber as the diaphragm, and 1.0 M sodium hexafluorophosphate (NaPF6) as the electrolyte. The entire battery assembly process must be carried out in an argon-protected glove box, and the oxygen concentration and water concentration in the glove box must be less than 1 ppm during assembly. The assembly order from bottom to top is the negative electrode of the battery shell, gasket, sodium metal sheet, diaphragm, homemade electrode sheet, gasket, and battery positive electrode shell. The electrolyte is dripped between the sodium metal sheet and the electrode sheet to fully infiltrate it. Finally, a hydraulic button cell packaging machine is used to seal the half-cell and let it stand for 12 hours to allow the electrolyte to completely infiltrate the interior of the battery. After the battery is assembled, the sodium ion battery performance is tested, and the results are as follows Figure 3 As shown, the results show that it exhibits good charge and discharge cycle performance and has extremely high stability.
[0039] The above embodiments are only preferred embodiments of the present invention and are not any formal or substantial limitations of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the present invention, and these improvements and supplements should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing ordered mesoporous carbon hollow flexible fibers, characterized in that: The following steps are involved: Step 1): preparing an electrospinning precursor solution containing a silicon source precursor and polyvinyl alcohol 1788, electrospinning the precursor solution to obtain a precursor fiber, and calcining the precursor fiber to obtain a flexible SiO2 fiber; The electrospinning precursor solution is prepared by mixing a silicon source precursor solution and a polyvinyl alcohol 1788 aqueous solution, and the silicon source precursor solution is prepared by a silicon source, an acid and a solvent; Step 2): Cut the SiO2 fiber obtained in step 1) into pieces and place them in an alkaline solvent, and stir and react with a silicon source, resorcinol and formaldehyde solution to prepare a flexible SiO2@SiO2@RF fiber; Step 3): drying the SiO2@SiO2@RF fiber obtained in step 2) and then carbonizing it to obtain a flexible SiO2@SiO2@C fiber; the carbonization treatment conditions are: heating to 600-1000°C at a heating rate of 1-3°C / min for 1-3 hours; Step 4): The SiO2@SiO2@C fibers obtained in step 3) are treated with alkaline solution to remove SiO2, and then washed and freeze-dried to obtain ordered mesoporous carbon hollow flexible fibers.
2. The method for preparing the ordered mesoporous carbon hollow flexible fiber according to claim 1, characterized in that: The silicon source is selected from at least one of tetramethyl orthosilicate, tetraethyl orthosilicate, tetrapropyl orthosilicate and tetrabutyl orthosilicate, and the acid is selected from at least one of phosphoric acid, formic acid and acetic acid.
3. The method for preparing ordered mesoporous carbon hollow flexible fibers according to claim 1, characterized in that: The alkaline solvent in step 2) is composed of ethanol, water and ammonia water; the silicon source is selected from at least one of tetramethyl orthosilicate, tetraethyl orthosilicate, tetrapropyl orthosilicate and tetrabutyl orthosilicate.
4. The method for preparing the ordered mesoporous carbon hollow flexible fiber according to claim 1, characterized in that: The molar ratio of the silicon source, resorcinol and formaldehyde in the step 2) is 4-6:1:1-2.
5. The method for preparing ordered mesoporous carbon hollow flexible fibers according to claim 1, characterized in that: The drying conditions in step 3) are: vacuum drying at 50-70° C. for 10-15 hours.
6. The method for preparing ordered mesoporous carbon hollow flexible fibers according to claim 1, characterized in that: The conditions of the alkali solution treatment in step 4) are: temperature 40-100° C., time 10-15 hours.
7. Ordered mesoporous carbon hollow flexible fibers prepared by the method for preparing ordered mesoporous carbon hollow flexible fibers according to any one of claims 1 to 6.
8. Use of the ordered mesoporous carbon hollow flexible fibers prepared by the method for preparing the ordered mesoporous carbon hollow flexible fibers according to any one of claims 1 to 7 in sodium ion batteries.