Preparation method of SGT structure
By adjusting the position of the source polysilicon through step-by-step etching and oxidation, the problem of excessive capacitance caused by the overlap of gate polysilicon and source polysilicon in SGT devices was solved, thereby reducing capacitance and improving performance.
Patent Information
- Application Number
- CN202310311454.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-03-28
AI Technical Summary
In the prior art, the overlap between the gate polysilicon and the source polysilicon of the SGT device results in a large capacitance Cgs, which affects the device performance.
The source polysilicon and field oxide layer are etched by a step-by-step etching process. An oxidation step is added before the second wet etching to form a sacrificial oxide layer. The position of the source polysilicon is adjusted to reduce overlap, and then the gate oxide layer is formed.
This effectively reduced the gate-source capacitance Cgs, lowered the input capacitance Ciss by 27%, and improved the electrical performance of the device.
Smart Images

Figure CN116387160B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor device manufacturing, and in particular to a method for preparing an SGT structure. Background Technology
[0002] In the field of medium and low voltage devices with a withstand voltage of 60V and above, shielded gate trench (SGT) devices are widely used due to their low specific on-resistance and low gate-drain coupling capacitance. The gate structure of an SGT device includes a shield polysilicon and a gate polysilicon, often referred to as the source polysilicon; both are formed within a trench. Depending on the arrangement of the shield and gate polysilicon within the trench, they are typically classified as either a top-bottom structure or a left-right structure. In the top-bottom structure, the shield polysilicon is located at the bottom of the trench, and the gate polysilicon is located at the top of the trench.
[0003] Currently, forming a polycrystalline silicon interlayer dielectric film (IPO) via thermal oxidation is a commonly used process in the upper and lower structures of medium-voltage SGTs. The specific manufacturing process is as follows: first, trenches 2 are etched into a silicon substrate 1; then, a field oxide layer 3 is deposited; next, source polycrystalline silicon 4 is filled into the trenches 2; and after defining the depth of the source polycrystalline silicon 4 using a dry process, the field oxide layer 3 formed on the sidewalls of the trenches 2 at a certain depth (e.g., ...) is removed. Figure 1 As shown), then a sacrificial oxide layer (not shown in the figure) and a gate oxide layer 5 (as shown in the figure) are formed. Figure 2 As shown), finally, the gate polysilicon 6 is deposited and etched back (as shown). Figure 3 (As shown). The above method utilizes highly doped source polysilicon, gate oxide (GOX), and polysilicon interlayer dielectric (IPO) film in a one-step process. However, this method has limitations on the gate oxide thickness, requiring a relatively thick gate oxide layer. Moreover, the resulting polysilicon interlayer dielectric film has poor morphology, and there is significant overlap between the gate polysilicon and source polysilicon, resulting in a large gate-source capacitance Cgs. Therefore, the gate-source capacitance Cgs, as a major component of the input capacitance Ciss of the SGT device, still has room for optimization. Summary of the Invention
[0004] In view of the shortcomings of the prior art described above, the purpose of this invention is to provide a method for fabricating an SGT structure to solve the problem that the capacitance Cgs increases due to the large overlap between the gate polysilicon and the source polysilicon.
[0005] To achieve the above and other related objectives, the present invention provides a method for preparing an SGT structure, the method comprising:
[0006] Step 1) Provide a semiconductor structure, the semiconductor structure including a semiconductor substrate with trenches, a field oxide layer formed on the surface of the trenches, and source polysilicon filled in the trenches;
[0007] Step 2) Etch the source polysilicon using a first etching process to retain the source polysilicon located at the bottom of the trench;
[0008] Step 3) The field oxide layer located on the upper part of the trench is etched by the second etching process to form a filling space in the trench, and the surface of the field oxide layer at the bottom of the filling space is lower than the top of the source polysilicon after the re-etching, wherein the upper sidewall of the trench retains a portion of the thickness of the field oxide layer.
[0009] Step 4) The source polysilicon is etched again by a third etching process so that the top of the source polysilicon after the second etching is lower than the surface of the field oxide layer located at the bottom of the filling space.
[0010] Step 5) The structure formed in step 4) is oxidized using an oxidation process to form a sacrificial oxide layer on the surface of the field oxide layer after the etch-back and on the surface of the source polysilicon after the etch-back.
[0011] Step 6) Remove the sacrificial oxide layer and the field oxide layer below it until the sidewall of the upper part of the trench is exposed, and make the surface of the field oxide layer at the bottom of the filling space lower than the top of the source polysilicon after the re-etching.
[0012] Step 7) A gate oxide layer is formed in the filling space, wherein the gate oxide layer covers the surface of the source polysilicon after the re-etching and the sidewall of the exposed upper part of the trench;
[0013] Step 8) Deposit polysilicon and etch back to form gate polysilicon.
[0014] Optionally, in step 2), the first etching process is a high selectivity isotropic dry etching.
[0015] Optionally, in step 3), the second etching process is wet etching.
[0016] Optionally, in step 4), the third etching process is an etching process combining isotropic dry etching and anisotropic dry etching.
[0017] Optionally, in step 4), the top of the source polysilicon after the re-etching is 800 to 1200 angstroms lower than the surface of the field oxide layer at the bottom of the filling space.
[0018] Optionally, in step 5), the oxidation process includes a low-temperature wet oxidation process.
[0019] Optionally, in step 5), the thickness of the sacrificial oxide layer formed is 600 angstroms to 800 angstroms.
[0020] Optionally, in step 6), the sacrificial oxide layer and the field oxide layer beneath it are removed by wet etching.
[0021] As described above, the method for fabricating the SGT structure of the present invention involves stepwise etching of the source polysilicon and the field oxide layer, and adding an oxidation step before the second wet etching to remove the field oxide layer. This results in the source polysilicon being slightly higher than the field oxide layers located on both sides before the formation of the gate oxide layer, thereby minimizing the overlap between the source polysilicon and the gate polysilicon. This improves the IPO morphology and reduces the Ciss capacitance. Furthermore, client testing results show that the Ciss capacitance of the SGT structure fabricated using the present invention is reduced by 27%. Attached Figure Description
[0022] Figure 1 The image shown is a scanning electron microscope (SEM) image of the SGT structure after the field oxide layer on the upper sidewall of the trench has been removed when the structure is prepared using existing methods.
[0023] Figure 2 Displayed as Figure 1 The image shown is a scanning electron microscope image of the structure after the formation of a sacrificial oxide layer and a gate oxide layer.
[0024] Figure 3 Displayed as Figure 2 The image shown is a scanning electron microscope (SEM) image of the structure after forming the gate polysilicon and then etching back.
[0025] Figure 4 The flowchart shown is a method for preparing the SGT structure of the present invention.
[0026] Figure 5 The image shown is a scanning electron microscope (SEM) image of the source polysilicon after being etched back using the first etching process according to the present invention.
[0027] Figure 6 The image shown is a scanning electron microscope (SEM) image of the field oxide layer after being etched back using the second etching process of the present invention.
[0028] Figure 7 The image shown is a scanning electron microscope (SEM) image of the source polysilicon after being re-etched using the third etching process of the present invention.
[0029] Figure 8 The image shown is a scanning electron microscope image of the sacrificial oxide layer formed according to the present invention.
[0030] Figure 9 The image shown is a scanning electron microscope image of the gate oxide layer formed according to the present invention.
[0031] Figure 10 The image shown is a scanning electron microscope (SEM) image of the gate polysilicon formed according to the present invention and after etch-back.
[0032] Explanation of icon numbers
[0033] 1: Silicon substrate; 10: Semiconductor structure; 2, 11: Trench; 111: Lower part of trench; 112: Upper part of trench; 12: Semiconductor substrate; 3, 13: Field oxide layer; 4, 14: Source polysilicon; 15: Fill space; 20: Sacrificial oxide layer; 5, 30: Gate oxide layer; 6, 40: Gate polysilicon Detailed Implementation
[0034] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.
[0035] Please see Figures 1 to 10 It should be noted that the illustrations provided in this embodiment are only schematic representations of the basic concept of the present invention. Although the illustrations only show components related to the present invention and are not drawn according to the actual number, shape and size of the components in the actual implementation, the shape, quantity and proportion of each component in the actual implementation can be arbitrarily changed, and the layout of the components may also be more complex.
[0036] like Figure 4 As shown, this embodiment provides a method for preparing an SGT structure, the method comprising:
[0037] Step 1) Provide a semiconductor structure 10, the semiconductor structure 10 including a semiconductor substrate 12 with trenches 11, a field oxide layer 13 formed on the surface of the trenches 11, and a source polysilicon 14 filled in the trenches 11;
[0038] Step 2) Etch the source polysilicon 14 using a first etching process to retain the source polysilicon 14 located in the lower part 111 of the trench;
[0039] Step 3) The field oxide layer 13 located in the upper part 112 of the trench is etched by the second etching process to form a filling space 15 in the trench 11, and the surface of the field oxide layer 13 located at the bottom of the filling space 15 is lower than the top of the source polysilicon 14 after the re-etching, wherein the sidewall of the upper part 112 of the trench retains a portion of the thickness of the field oxide layer 13;
[0040] Step 4) The source polysilicon 14 is etched again by a third etching process so that the top of the source polysilicon 14 after the second etching is lower than the surface of the field oxide layer 13 located at the bottom of the filling space 15.
[0041] Step 5) The structure formed in step 4) is oxidized using an oxidation process to form a sacrificial oxide layer 20 on the surface of the field oxide layer 13 after the etch-back and on the surface of the source polysilicon 14 after the etch-back.
[0042] Step 6) Remove the sacrificial oxide layer 20 and the field oxide layer 13 below it until the sidewall of the upper part 112 of the trench is exposed, and make the surface of the field oxide layer 13 at the bottom of the filling space 15 lower than the top of the source polysilicon 14 after the re-etching.
[0043] Step 7) A gate oxide layer 30 is formed in the filling space 15, wherein the gate oxide layer 30 covers the surface of the source polysilicon 14 after being etched back and the sidewall of the exposed upper part 112 of the trench;
[0044] Step 8) Deposit polysilicon and etch back to form gate polysilicon 40.
[0045] The preparation method of the SGT structure provided in this embodiment will be described in detail below with reference to the accompanying drawings.
[0046] like Figure 5 As shown, in step 1), a semiconductor structure 10 is provided, the semiconductor structure 10 including a semiconductor substrate 12 with trenches 11, a field oxide layer 13 formed on the surface of the trenches 11, and a source polysilicon 14 filled in the trenches 11.
[0047] In this embodiment, the field oxide layer 13 extends beyond the bottom and sidewalls of the trench 11 to the surface of the semiconductor substrate 12 (i.e., the area where the trench 11 is not formed), and the material of the field oxide layer 13 includes silicon oxide. In this embodiment, the semiconductor substrate 12 includes, but is not limited to, a silicon substrate or a silicon-on-insulator substrate.
[0048] like Figure 5As shown, in step 2), the source polysilicon 14 is etched by a first etching process to retain the source polysilicon 14 located in the lower part 111 of the trench.
[0049] In this embodiment, for low-voltage SGT devices, the depth of the source polysilicon 14 removed by the first etching process is 0.2 to 0.25 times the depth of the trench 11.
[0050] Specifically, in step 2), the first etching process is a high-selectivity isotropic dry etching. In this embodiment, by employing an isotropic dry etching process, the source polysilicon 14 after etching back can have a better morphology.
[0051] like Figure 6 As shown, in step 3), the field oxide layer 13 located on the upper part 112 of the trench is etched by a second etching process to form a filling space 15 in the trench 11, and the surface of the field oxide layer 13 located at the bottom of the filling space 15 is lower than the top of the source polysilicon 14 after the re-etching, wherein the sidewall of the upper part 112 of the trench retains a portion of the thickness of the field oxide layer 13.
[0052] In this embodiment, after the field oxide layer 13 is etched by the second etching process, the source polysilicon 14 after being etched back extends from the surface of the field oxide layer 13 at the bottom of the filling space 15 to form an extension.
[0053] Specifically, in step 3), the second etching process is wet etching.
[0054] In this embodiment, when the field oxide layer 13 is etched by wet etching, the purpose of retaining a portion of the thickness of the field oxide layer 13 on the sidewall of the upper part 112 of the trench is to protect the semiconductor substrate 12 in subsequent processes.
[0055] like Figure 7 As shown, in step 4), the source polysilicon 14 is etched again by a third etching process so that the top of the source polysilicon 14 after the second etching is lower than the surface of the field oxide layer 13 located at the bottom of the filling space 15.
[0056] Specifically, in step 4), the third etching process is an etching process that combines isotropic dry etching and anisotropic dry etching.
[0057] In this embodiment, the source polysilicon 14 is re-etched by combining isotropic dry etching and anisotropic dry etching, so that the source polysilicon 14 after re-etching has a better morphology.
[0058] As an example, in step 4), the top of the source polysilicon 14 after being etched back is 800 to 1200 angstroms lower than the surface of the field oxide layer 13 at the bottom of the filling space 15.
[0059] like Figure 8 As shown, in step 5), the structure formed in step 4) is oxidized using an oxidation process to form a sacrificial oxide layer 20 on the surface of the field oxide layer 13 after etch-back and on the surface of the source polysilicon 14 after etch-back again.
[0060] In this embodiment, the material of the sacrificial oxide layer 20 is the same as that of the field oxide layer 13. Therefore, in the scanning electron microscope image, the sacrificial oxide layer 20 formed on the surface of the field oxide layer 13 is not distinguished from the field oxide layer 13. Furthermore, this embodiment employs a low-temperature wet oxidation process to generate a thicker sacrificial oxide layer 20. This allows the top of the source polysilicon 14 after etching back to protrude above the surface of the remaining field oxide layer 13 located at the bottom of the filling space 15 after the sacrificial oxide layer 20 is removed.
[0061] Specifically, in step 5), the oxidation process includes a low-temperature wet oxygen oxidation process. In this embodiment, the temperature of the low-temperature wet oxygen oxidation process is 800°C.
[0062] As an example, in step 5), the thickness of the sacrificial oxide layer 20 formed is 600 angstroms to 800 angstroms.
[0063] In step 6), the sacrificial oxide layer 20 and the field oxide layer 13 below it are removed until the sidewall of the upper part 112 of the trench is exposed, and the surface of the field oxide layer 13 at the bottom of the filling space 15 is lower than the top of the source polysilicon 14 after being etched back.
[0064] Specifically, in step 6), the sacrificial oxide layer 20 and the field oxide layer 13 below it are removed by wet etching.
[0065] like Figure 9 As shown, in step 7), a gate oxide layer 30 is formed in the filling space, wherein the gate oxide layer 30 covers the surface of the source polysilicon 14 after being etched back and the sidewall of the exposed upper part 112 of the trench.
[0066] In this embodiment, the gate oxide layer 30 and the IPO (polysilicon interlayer dielectric film) are formed using the same process steps. Specifically, the gate oxide layer 30 formed on the surface of the source polysilicon 14 after the re-etching is used as the IPO.
[0067] like Figure 10As shown, in step 8), polysilicon is deposited and etched back to form gate polysilicon 40.
[0068] In summary, the SGT structure fabrication method of this invention, by performing stepwise etching of the source polysilicon and the field oxide layer, and adding an oxidation step before the second wet etching to remove the field oxide layer, ensures that the source polysilicon is slightly higher than the field oxide layers on both sides before the formation of the gate oxide layer. This minimizes the overlap between the source polysilicon and the gate polysilicon, thereby improving the IPO morphology and reducing Ciss capacitance. Moreover, client-side testing results show that the Ciss capacitance of the SGT structure fabricated using this invention is reduced by 27%. Therefore, this invention effectively overcomes the various shortcomings of the prior art and has high industrial applicability.
[0069] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.
Claims
1. A method for preparing an SGT structure, characterized in that, The method includes: Step 1) Provide a semiconductor structure, the semiconductor structure including a semiconductor substrate with trenches, a field oxide layer formed on the surface of the trenches, and source polysilicon filled in the trenches; Step 2) Etch the source polysilicon using a first etching process to retain the source polysilicon located at the bottom of the trench; Step 3) The field oxide layer located on the upper part of the trench is etched by the second etching process to form a filling space in the trench, and the surface of the field oxide layer at the bottom of the filling space is lower than the top of the source polysilicon after the re-etching, wherein the upper sidewall of the trench retains a portion of the thickness of the field oxide layer. Step 4) The source polysilicon is etched again by a third etching process so that the top of the source polysilicon after the second etching is lower than the surface of the field oxide layer located at the bottom of the filling space. Step 5) The structure formed in step 4) is oxidized using an oxidation process to form a sacrificial oxide layer on the surface of the field oxide layer after the etch-back and on the surface of the source polysilicon after the etch-back. Step 6) Remove the sacrificial oxide layer and the field oxide layer below it until the sidewall of the upper part of the trench is exposed, and make the surface of the field oxide layer at the bottom of the filling space lower than the top of the source polysilicon after the re-etching. Step 7) A gate oxide layer is formed in the filling space, wherein the gate oxide layer covers the surface of the source polysilicon after the re-etching and the sidewall of the exposed upper part of the trench; Step 8) Deposit polysilicon and etch back to form gate polysilicon.
2. The method for preparing the SGT structure according to claim 1, characterized in that, In step 2), the first etching process is a high selectivity isotropic dry etching.
3. The method for preparing the SGT structure according to claim 1, characterized in that, In step 3), the second etching process is wet etching.
4. The method for preparing the SGT structure according to claim 1, characterized in that, In step 4), the third etching process is an etching process that combines isotropic dry etching and anisotropic dry etching.
5. The method for preparing the SGT structure according to claim 4, characterized in that, In step 4), the top of the source polysilicon after the re-etching is 800 to 1200 angstroms lower than the surface of the field oxide layer at the bottom of the filling space.
6. The method for preparing the SGT structure according to claim 1, characterized in that, In step 5), the oxidation process includes a low-temperature wet oxygen oxidation process.
7. The method for preparing the SGT structure according to claim 6, characterized in that, In step 5), the thickness of the sacrificial oxide layer formed is 600 angstroms to 800 angstroms.
8. The method for preparing the SGT structure according to claim 1, characterized in that, In step 6), the sacrificial oxide layer and the field oxide layer beneath it are removed by wet etching.
Citation Information
Patent Citations
Shield gate trench type transistor and manufacturing method thereof
CN110838448A
Shielded gate type metal-oxide-semiconductor field effect transistor and manufacturing method thereof
CN110957357A