A hydrogen sulfide selective oxidation desulfurization catalyst and preparation method thereof

Through the magnesium-manganese spinel composite metal oxide catalyst, the problems of poor durability and low selectivity of manganese-based materials are solved, efficient H2S selective oxidation and stability are achieved, and the performance of the catalyst is significantly improved.

CN116393121BInactive Publication Date: 2024-11-08FUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310422498.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing H2S selective catalytic oxidation catalysts have problems of poor durability and low selectivity, especially the low electron transport efficiency and unstable activity of manganese-based materials, which leads to rapid inactivation under high temperature conditions.

Method used

The magnesium-manganese spinel composite metal oxide catalyst is used to enter the trimanganese tetraoxide lattice of the spinel phase through magnesium elements, replace the original Mn2+ site, and prepare a sponge-like morphology and relatively Large pore size catalysts improve oxygen mobility and storage capacity of elemental sulfur.

Benefits of technology

High activity and stability are achieved, the H2S conversion rate of the catalyst can reach 99% at 150°C, and the conversion rate is maintained above 88% at 180°C, which significantly improves the durability and selectivity of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116393121B_ABST
    Figure CN116393121B_ABST
Patent Text Reader

Abstract

The invention discloses a hydrogen sulfide selective oxidation desulfurization catalyst and a preparation method thereof, belonging to the technical field of material preparation and environmental catalysis. The catalyst is prepared by an improved sol-gel method: magnesium salt and manganese salt are dissolved in alcohol at a fixed ratio, a complexing agent dissolved in an alcohol solution is added, and then heated in a water bath, stirred, dried and calcined to obtain a magnesium-manganese composite metal oxide (MgMn) having a spinel phase. 2 O 4 ) catalyst, and is used in the selective oxidative desulfurization reaction of hydrogen sulfide. The magnesium manganese spinel catalyst prepared by the method provided by the present invention has a high specific surface area and a large pore size, and is used in the selective catalytic oxidation of H 2 In the S reaction, at 150°C, the conversion rate reached 99.8%, the sulfur selectivity was higher than 99%, and it showed good stability, which is conducive to promotion and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material preparation and environmental catalysis, and particularly relates to a hydrogen sulfide selective oxidation desulfurization catalyst and a preparation method thereof. Background Art

[0002] The coal chemical industry inevitably produces a large amount of sulfur-containing waste gas, including carbonyl sulfide (COS), hydrogen sulfide (H2S), sulfur dioxide (SO2) and various sulfur-containing organic compounds. Currently, the most commonly used and largest-scale desulfurization process is the Claus process, which is used to remove H2S and recover sulfur resources. Due to thermodynamic limitations, 2-5% H2S will still remain in the flue gas after the Claus process. In recent years, the selective catalytic oxidation (SCO) of H2S has received extensive research attention for the efficient and deep removal and resource utilization of H2S in the tail gas of the Claus process. It directly catalytically oxidizes H2S to produce elemental sulfur and is not limited by thermodynamic equilibrium. However, the accompanying side reaction produces SO2, which reduces the sulfur yield. The main reaction of SCO is shown in equation (1), and the side reactions are shown in (2) and (3).

[0003]

[0004] The deep oxidation of H2S and the further oxidation of S in the reaction will both form SO2, resulting in a decrease in sulfur yield. Therefore, the development of highly active, highly selective and highly durable catalysts is an urgent problem to be solved in the selective catalytic oxidation of H2S.

[0005] The catalyst of H2S selective catalytic oxidation technology should prevent the reverse Claus reaction and deep oxidation of elemental sulfur to form SO2. The temperature of selective catalytic oxidation can be higher or lower than the sulfur dew point (180 ℃). When the temperature is above the sulfur dew point, it is a continuous process, while when the temperature is below the sulfur dew point, it is an intermittent process. The elemental sulfur formed in the intermittent process is concentrated and deposited in the pore structure of the catalyst, and regular regeneration is required to remove the deposited sulfur. Therefore, the catalyst should have a dual role: it is both a catalyst for direct oxidation of H2S and an adsorbent for removing sulfur by chemical adsorption, and keeping it in the pore structure for easy handling of the desulfurizer. At present, the work carried out on H2S selective catalytic oxidation catalysts is mainly distributed in metal oxides, carbon materials and pillared clay systems. Among them, carbon materials have abundant pores and easily modified surface sites, but the disadvantages of carbon materials as catalysts are low application space velocity and low selectivity; when carbon materials are used as carriers, there is a problem of loss of active components; pillared clay systems show good activity, but poor durability and stability. Metal oxide catalysts are the most studied and used catalysts in the process of H2S selective catalytic oxidation. They have attracted much attention due to their relatively simple preparation and high activity. Metal oxide catalysts can usually operate at relatively high H2S concentrations and mass space velocities. The reaction hydrogen sulfide concentration can reach 5000 ppm, and a few metal oxides can operate at mass space velocities of more than 20000 mL / g / h. Usually, transition metal and alkaline earth metal oxides can show good catalytic activity, and their activity order can be expressed as: V2O5>Mn2O3>CoO>TiO2>Fe2O3>Bi2O3>Sb6O 13 >CuO>Al2O3= MgO = Cr2O3, among which the most common ones are TiO2, Fe2O3 and V2O5. Titanium-based catalysts have the advantages of high temperature activity and good stability, but they are easily affected by water in the system and have poor water resistance. Pure iron oxide catalysts have good H2S conversion rates under oxygen-rich conditions but poor sulfur selectivity and low durability. Vanadium-based catalysts have the best activity but their strong toxicity greatly limits their application. Among transition metal oxide catalysts, manganese-based catalysts have received high attention due to their rich chemical states and high activity. In existing literature reports, the lower electron transfer efficiency and specific surface area of ​​manganese-based materials make them less durable and selective as H2S selective oxidation desulfurization catalysts, and their rapid deactivation limits their application. Summary of the invention

[0006] The purpose of the present invention is to solve the problems of poor durability and low selectivity of Mn2O3 materials, and provide a magnesium-manganese spinel composite metal oxide catalyst and its preparation method and application, by using magnesium element to enter the spinel phase of manganese tetraoxide lattice to replace the original Mn 2+site, exploring the application of magnesium manganese spinel catalysts in the field of H2S selective catalytic oxidation. The higher electron transfer efficiency of magnesium manganese spinel is more likely to induce the formation of surface oxygen vacancies, improve oxygen mobility and thus obtain good redox performance. At the same time, the larger pore size also increases the storage capacity of elemental sulfur, reduces the deactivation caused by elemental sulfur accumulation, and thus improves the catalytic activity and stability.

[0007] To achieve the above object, the present invention adopts the following technical solution:

[0008] A method for preparing a hydrogen sulfide selective oxidation desulfurization catalyst comprises the following steps:

[0009] a. Dissolve the magnesium salt and manganese salt in alcohol and stir at room temperature for 15 minutes to obtain a magnesium-manganese mixed salt alcohol solution A;

[0010] b. The complexing agent was added to the alcohol solution and stirred at room temperature for 10 min to obtain a complexing agent alcohol solution B, and then the B solution was added to the A solution to obtain a mixed solution C;

[0011] c. Heat solution C in a water bath and stir vigorously for 4-12 hours, until the solution becomes gel-like, and dry for 8-12 hours;

[0012] d. The dried material was heated to 400-800°C at a heating rate of 2°C / min and calcined for 3 hours to obtain a magnesium-manganese composite metal oxide catalyst having a spinel phase.

[0013] In step a, the molar ratio of Mg to Mn is 0.5-0.9:1, and the total molar concentration of Mg and Mn in the magnesium-manganese mixed alcohol solution is 0.2-0.5 mol / L; the magnesium salt is at least one of magnesium nitrate, magnesium acetate, and magnesium chloride; the manganese salt is at least one of manganese nitrate, manganese acetate, and manganese chloride; and the alcohol is at least one of ethanol, ethylene glycol, and polyethylene glycol.

[0014] The complexing agent described in step b is at least one of citric acid and tartaric acid; the alcohol is at least one of ethanol, ethylene glycol, and polyethylene glycol, which is consistent with the alcohol used in step a, and the volume ratio of deionized water to alcohol in the alcohol solution is 1-2:1; the molar concentration of the complexing agent alcohol solution is 0.05-0.25 mol / L.

[0015] In step c, the water bath heating temperature is 60-90°C, and the drying temperature is 60-120°C.

[0016] An application of a hydrogen sulfide selective oxidation desulfurization catalyst prepared by the method as described above; a magnesium-manganese composite metal oxide catalyst with a spinel phase is used for selective catalytic oxidation of H2S, the reaction temperature is 90-210°C, the amount of the catalyst is 0.15g; the particle size of the catalyst is 30-80 mesh; the raw gas components and contents are: 5000 ppm H2S and 2500ppm O2, N2 is the balance gas; the reaction mass space velocity is 12000mL / g / h; the raw gas flow rate is 30mL / min.

[0017] Compared with the prior art, the beneficial effects of the present invention are:

[0018] (1) The present invention applies spinel-phase magnesium-manganese composite metal oxide (MgMn2O4) to the field of H2S selective catalytic oxidation for the first time, thus expanding the application scenarios of magnesium-manganese composite metal oxide;

[0019] (2) The present invention utilizes the sol-gel method and uses specific alcohols as solvents, so that the final obtained composite metal oxide has a special sponge-like morphology and a larger pore size of 11 to 20 nm. The larger pore size is conducive to the discharge of the accumulated sulfur element, thereby achieving high durability;

[0020] (3) The magnesium-manganese composite metal oxide prepared by the present invention achieves a large capacity for H2S adsorption. Under the conditions of 30°C and a raw gas flow rate of 30 mL / min, effective adsorption is achieved for 26 minutes and penetration is achieved in about 26 minutes. Under the conditions of 150°C and a raw gas flow rate of 30 mL / min, 99% conversion of H2S can be stably achieved. Under the conditions of 180°C and a raw gas flow rate of 30 mL / min, the stability test is carried out for 98 hours, and the conversion rate of H2S can be maintained above 88%. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The SEM images of the magnesium-manganese composite metal oxides prepared in Examples 1 to 5 of the present invention; Figure 1 (a) is a MgMn2O4-400 catalyst; Figure 1 (b) is a MgMn2O4-500 catalyst; Figure 1 (c) is a MgMn2O4-650 catalyst; Figure 1 (d) is a MgMn2O4-800 catalyst; Figure 1 (e) is a MgMn2O4-TA catalyst;

[0022] Figure 2 It is a curve diagram of the conversion rate of selective catalytic oxidation of H2S in the temperature range of 90-210°C for the catalysts prepared in Examples 1-5 of the present invention and Comparative Example 1;

[0023] Figure 3 The sulfur selectivity curve of the catalysts prepared in Examples 1 to 5 of the present invention and Comparative Example 1 for selective catalytic oxidation of H2S in the temperature range of 90 to 210°C;

[0024] Figure 4 This is a stability curve of the catalyst prepared in Example 1 of the present invention for selective catalytic oxidation of H2S at a temperature of 180°C. DETAILED DESCRIPTION

[0025] In order to make the contents of the present invention easier to understand, the technical solution of the present invention is further described below in conjunction with specific implementation methods, but the present invention is not limited thereto.

[0026] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources;

[0027] The quantitative tests in the following examples were all repeated three times, and the results were averaged.

[0028] The experimental methods in the following embodiments are conventional methods unless otherwise specified.

[0029] Example 1

[0030] Weigh 0.01 mol of magnesium nitrate hexahydrate and 0.02 mol of 50% manganese nitrate solution, add them to 150 mL of anhydrous ethanol, and stir at room temperature for 10 min. Then add 0.03 mol of citric acid monohydrate to a mixed solution of 75 mL of deionized water and 75 mL of anhydrous ethanol, and stir and dissolve at room temperature to obtain a complexing agent solution. Add the complexing agent solution to the mixed salt solution, stir and heat in a water bath at 85 ° C until the solution is gel-like. Then transfer the system to an oven and bake at 120 ° C for 12 h. After waiting for the fluffy sample to cool in dry air, heat it to 400 ° C in a muffle furnace at a heating rate of 2 ° C / min for 3 h to obtain a catalyst, named MgMn2O4-400.

[0031] Example 2

[0032] The difference between Example 2 and Example 1 is that the high temperature calcination temperature in the muffle furnace is 500°C, and the catalyst is obtained after calcination for 3 hours, and is named MgMn2O4-500;

[0033] Example 3

[0034] The difference between Example 3 and Example 1 is that the high-temperature calcination temperature in the muffle furnace is 650° C., and the catalyst is obtained after calcination for 3 hours, and is named MgMn2O4-650.

[0035] Example 4

[0036] The difference between Example 4 and Example 1 is that the high-temperature calcination temperature in the muffle furnace is 800° C., and the catalyst is obtained after calcination for 3 hours, and is named MgMn2O4-800.

[0037] Example 5

[0038] Weigh 0.01 mol of magnesium nitrate hexahydrate and 0.02 mol of 50% manganese nitrate solution, add them to 150 mL of anhydrous ethanol, and stir at room temperature for 10 min. Then add 0.03 mol of tartaric acid to a mixed solution of 75 mL of ethylene glycol and 75 mL of anhydrous ethanol, and stir and dissolve at room temperature to obtain a complexing agent solution. Add the complexing agent solution to the mixed salt solution, stir and heat in a water bath at 85 ° C until the solution is gel-like. Then transfer the system to an oven and bake at 120 ° C for 12 h. After waiting for the fluffy sample to cool in dry air, heat it to 400 ° C in a muffle furnace at a heating rate of 2 ° C / min for 3 h to obtain a catalyst, named MgMn2O4-TA.

[0039] Comparative Example 1

[0040] Weigh 0.03 mol of 50% manganese nitrate solution, add it to 150 mL of anhydrous ethanol, and stir at room temperature for 10 minutes. Then add 0.03 mol of monohydrated citric acid to a mixed solution of 75 mL of deionized water and 75 mL of anhydrous ethanol, and stir to dissolve at room temperature. Add the complexing agent solution to the mixed salt solution, and heat it in a water bath at 85 ° C with stirring until the solution is gel-like. Then transfer the system to an oven and bake it at 120 ° C for 12 hours. After waiting for the fluffy sample to cool in dry air, heat it to 400 ° C in a muffle furnace at a heating rate of 2 ° C / min for 3 hours to obtain a catalyst, named Mn2O3-400. Figure 1 The SEM images of the magnesium-manganese composite metal oxides prepared in Examples 1 to 5 of the present invention are shown in FIG. Figure 1 In the experiment, the calcination temperature greatly affects the material structure of the catalyst. The change of calcination temperature shows obvious differences in morphological characteristics. With the increase of calcination temperature, the fluffy sponge structure of the catalyst gradually collapses and sinters, forming an agglomerated polyhedron structure of 10-20nm.

[0041] As shown in Table 1, the catalyst texture parameters prepared by Examples 1 to 5 of the present invention and Comparative Example 1 are shown. As can be seen from Table 1, as the calcination temperature increases, the specific surface area of ​​the sample gradually decreases, and decreases in the order of MgMn2O4-400>MgMn2O4-TA>Mn2O3-400>MgMn2O4-500>MgMn2O4-650>MgMn2O4-800. As magnesium enters the unit cell skeleton, the specific surface area and mesopore volume of the sample both increase first and then decrease, which is beneficial to the adsorption of H2S on the catalyst surface and in the pores, increasing the chance of contact of active sites, thereby obtaining a good H2S conversion rate and catalytic durability.

[0042]

[0043] Figure 2 The conversion rate curve of the catalyst prepared by Examples 1 to 5 of the present invention and Comparative Example 1 in the selective catalytic oxidation of H2S in the temperature range of 90 to 210°C. The conversion rate of H2S gradually increases with the increase of temperature. As the calcination temperature increases, the H2S conversion rate of the corresponding sample gradually decreases. At 150°C, the H2S conversion rate of the MgMn2O4-400 sample is close to 100%. Under the same reaction conditions in the low temperature section, MgMn2O4-400 exhibits better performance than Mn2O3-400 and has a higher conversion rate.

[0044] Figure 3 The sulfur selectivity curve of the catalyst prepared in Examples 1 to 5 of the present invention and Comparative Example 1 for selective catalytic oxidation of H2S in the temperature range of 90 to 210°C is shown. For the Mn2O3-400 sample, there is a significant decrease in selectivity as the temperature increases, while the MgMn2O4-400 still maintains a high selectivity of 99% at 150°C, and even after the temperature is increased to 210°C, the selectivity remains above 93%. In general, the selectivity shows a trend of decreasing with the increase of the calcination temperature, and the selectivity order at 150°C is MgMn2O4-400>MgMn2O4-500>MgMn2O4-TA>MgMn2O4-650>MgMn2O4-800>Mn2O3-400.

[0045] Figure 4The stability curve of the selective catalytic oxidation of H2S at a temperature of 180°C for the catalyst prepared in Example 1 of the present invention. 180°C is the sulfur dew point temperature, and the catalytic oxidation is a continuous process when it is operated at a temperature above the sulfur dew point. Specifically, the H2S conversion rate of the MgMn2O4-400 catalyst in the first 24 hours is close to 100%. Although there is a slight decrease in activity around 40 hours, the conversion rate is still maintained at more than 95%. After 98 hours of stability testing, the conversion rate remained above 88.6%. The sulfur selectivity was always higher than 95% during the entire stability test.

[0046] In summary, the magnesium-manganese composite metal oxide prepared by the present invention has excellent catalytic stability and catalytic performance in the field of selective catalytic oxidation of H2S.

[0047] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.

Claims

1. A method for preparing a hydrogen sulfide selective oxidation desulfurization catalyst, characterized in that: The following steps are involved: a. dissolving magnesium salt and manganese salt in alcohol, stirring at room temperature for 15 minutes, to obtain a magnesium-manganese mixed salt alcohol solution A; the alcohol is at least one of ethanol, ethylene glycol, and polyethylene glycol; the molar ratio of Mg to Mn is 0.5-0.9:1, and the total molar concentration of Mg and Mn in the magnesium-manganese mixed alcohol solution is 0.2-0.5 mol / L; b. The complexing agent is added to the alcohol solution, stirred at room temperature for 10 min to obtain a complexing agent alcohol solution B, and then the solution B is added to the solution A to obtain a mixed solution C; the complexing agent is at least one of citric acid and tartaric acid; c. Heat solution C in a water bath and stir vigorously for 4-12 hours, until the solution becomes gel-like, and dry for 8-12 hours; d. The dried material was heated to 400-800°C at a heating rate of 2°C / min and calcined for 3 hours to obtain a magnesium-manganese composite metal oxide catalyst having a spinel phase.

2. The method according to claim 1, characterized in that: The magnesium salt described in step a is at least one of magnesium nitrate, magnesium acetate and magnesium chloride; the manganese salt is at least one of manganese nitrate, manganese acetate and manganese chloride.

3. The method according to claim 1, characterized in that: The alcohol described in step b is at least one of ethanol, ethylene glycol, and polyethylene glycol, which is consistent with the alcohol used in step a. The volume ratio of deionized water to alcohol in the alcohol solution is 1-2:1; the molar concentration of the complexing agent alcohol solution is 0.05-0.25 mol / L.

4. The method according to claim 1, characterized in that: In step c, the water bath heating temperature is 60-90°C, and the drying temperature is 60-120°C.

5. A catalyst for selective oxidation desulfurization of hydrogen sulfide obtained by the method according to any one of claims 1 to 4.

6. An application of a catalyst for selective oxidation desulfurization of hydrogen sulfide prepared by the method according to any one of claims 1 to 4, characterized in that: A magnesium-manganese composite metal oxide catalyst having a spinel phase is used for the selective catalytic oxidation of H2S.