Aluminate glass and its preparation method and application

By optimizing the aluminate glass formula and preparation method, the problem of insufficient thermal shock resistance of existing infrared transmission materials in high-speed aircraft was solved, and aluminates with high transmittance, thermal shock resistance and chemical stability were prepared. Glass is suitable for complex shapes and high-temperature environments, reducing costs and broadening the scope of applications.

CN116395959BActive Publication Date: 2024-10-22LUMISING SPECIAL GLASS TECH CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202310259016.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-17
Publication Date
2024-10-22
Estimated Expiration
2043-03-17

AI Technical Summary

Technical Problem

Existing infrared-transmitting materials have insufficient thermal shock resistance in high-speed aircraft, have high processing costs, and are prone to crystallization, making it difficult to meet the high temperature and complex shape requirements of high-speed aircraft.

Method used

Using optimized aluminate glass formula and preparation method, through high-temperature burning dehydration treatment, atmosphere-protected melting and rapid cooling molding, aluminate glass is prepared that is not easy to crystallize, has high hardness and high infrared transmittance, and is suitable for complex applications. Shape processing and molding preparation of shapes.

Benefits of technology

It achieves high transmittance, thermal shock resistance and chemical stability in the mid-infrared band, reduces material costs, broadens the application range of aluminate glass, and is suitable for infrared-transmitting shields, optical windows and high-temperature fairings and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004130515500000031
    Figure BDA0004130515500000031
  • Figure BDA0004130515500000042
    Figure BDA0004130515500000042
  • Figure BDA0004130515500000043
    Figure BDA0004130515500000043
Patent Text Reader

Abstract

The invention discloses an aluminate glass and a preparation method and application thereof. The aluminate glass consists of the following components in percentage by weight: 38-45% Al2O3, 0.1-1% Na2O, 36-43% CaO, 0.1-1% MgO, 0.5-3.9% SrO, 0.5-3.9% BaO, 1-10% Gd2O3, 0.5-5% GeO2, 0.1-1% ZrO2, 0.5-4.9% ZnO, 0.1-1% Ga2O3 and 0.1-2.5% TiO2. The present invention also provides a method for preparing aluminate glass, comprising the following steps: (1) glass batching: firstly subjecting the glass raw materials to a high-temperature burning and dehydration treatment, and then weighing each raw material according to the weight percentage of each component; (2) glass melting: placing the mixture into a platinum crucible, and then placing it into a glass melting furnace at 1460°C-1600°C for heating for 4 to 8 hours, and introducing dry argon gas during the melting process; (3) rapid cooling and forming: after the glass is evenly melted, pouring the molten glass liquid into a preheated mold and casting it into a specified specification, and then placing it in an annealing furnace for annealing, cooling it to room temperature with the furnace, and cooling to obtain an aluminate glass material. The aluminate glass prepared by the present invention can be used to prepare infrared-transmitting optical devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of special glass materials and preparation thereof, and in particular to aluminate glass and a preparation method and application thereof. Background Art

[0002] Infrared is an electromagnetic wave with a wavelength between microwaves and visible light, ranging from 0.75μm to 500μm. It is a non-visible light with a longer wavelength than red light, and has the characteristics of thermal effect, invisible to the naked eye, and strong ability to penetrate clouds and fog. Infrared can be divided into three parts, namely near infrared (wavelength range of 0.75μm to 2.5μm), mid-infrared (wavelength range of 2.5μm to 25μm), and far infrared (wavelength range of 25μm to 500μm). Infrared has a wide range of uses in electronic communications, remote sensing testing, industrial detection, environmental monitoring, biomedicine, national defense and military.

[0003] At present, the research focus of infrared optical materials at home and abroad is on materials in the 1-5μm band, because the infrared rays in the 1-5μm band have the least attenuation in the atmosphere. In order to increase the infrared-transmitting monitoring sensing range, the infrared-transmitting materials are preferably processed into a round cover shape. Taking fire warning as an example, the fire sensor has a good transmittance for infrared rays with a wavelength of 1.0-5.0μm through the round cover-shaped infrared-transmitting cover. Fire alarms are installed in theaters, stadiums, conference venues, tunnels and culverts to sense the occurrence of fires. They are mainly sensed by infrared rays emitted by flames, and the reaction speed is fast. Especially in the vast space of large buildings, the infrared sensing is faster and more reliable than the sensing of smoke and combustion products. Flame is a hot heat source generated by the combustion reaction. Due to the addition of smoke and combustion products, it becomes very complicated and can emit infrared light. Among the light energy emitted by the flame, the luminescence in the infrared range is unique to the flame. Therefore, the infrared transparent material must be highly sensitive to the infrared rays unique to the flame, and its infrared wavelength perception range is in the 1.0-5.0μm band range; others such as missile guidance outer covers also use the same principle. The manufacturing material of the missile head fairing requires good infrared transparent material performance, can withstand 800℃ high temperature, and have good temperature resistance and strain performance. This is because when the missile is launched, the head material is rubbed by the airflow, which will cause the surface temperature to rise suddenly in a very short time, and the material is required not to break or deform. Therefore, the infrared transparent material should have good thermal shock resistance. In addition, in order to adapt to the field environment, the infrared transparent material is required to have good chemical stability and mechanical strength.

[0004] At present, the infrared-transmitting cover materials used for 1μm to 5μm mid-infrared rays mainly include ZnS, spinel, sapphire, and infrared optical glass. Although these materials have advantages in some performance aspects and can be used as general infrared window materials, they still have various deficiencies in heat shock resistance for infrared covers of high-speed aircraft. For example, ZnS has high infrared transmittance and is easy to be processed into the required window or cover shape, but the ZnS material itself is very soft and is extremely easy to be worn under normal conditions, which limits its application range and service life. In actual use, it can be improved by coating a protective film, but the high temperature generated by friction with the air during the high-speed flight of missiles or rockets will cause the plated film layer to fall off. The infrared transmittance of spinel is slightly worse than that of ZnS. It has partial absorption at a wavelength of 5μm, but its hardness is more than ten times that of ZnS, and its fracture toughness is higher, so it has strong heat shock resistance, but spinel is difficult to form and process into a window or cover, and the material and processing costs are very high. The infrared transmittance of sapphire is the same as that of spinel, and its hardness and fracture toughness are 40% higher than those of spinel. Windows and covers made of sapphire are highly wear-resistant and can be used in supersonic applications. However, the manufacturing cost of this material is high and its hardness makes it difficult to process and shape, making the processing cost very expensive.

[0005] Infrared optical glass mainly includes quartz glass, germanate glass, tellurite glass, chalcogenide glass and aluminate glass. Among them, quartz glass has excellent spectral characteristics, is transparent to both infrared and ultraviolet, and has high visible light transmittance. However, the melting temperature of quartz glass is high and it is easy to absorb water, which reduces its transmittance in the near-infrared region. In addition, due to the strong Si-O bond, its infrared transmittance cutoff limit is small, which limits the application of quartz glass. Germanate glass has good infrared transmittance, but its mechanical properties are poor. The poor chemical stability, high thermal expansion coefficient and low softening temperature of tellurite glass limit its application. The long-wave limit of chalcogenide glass is cutoff at 10μm, but chalcogenide glass has very high requirements on the purity of raw materials, and the melting must be carried out under vacuum or inert gas conditions. In addition, the defects of chalcogenide glass such as low hardness, low softening temperature and large expansion coefficient also limit its application. Aluminate glass is mainly an infrared glass with aluminum oxide and calcium oxide as the main components. Aluminate glass has the advantages of excellent temperature strain resistance, high mechanical properties, and high glass softening temperature. It is the preferred material for manufacturing high-temperature fairings. 2 O 3 -CaO binary phase diagram shows that 12CaO·7Al 2 O 3 Glass can be formed in a narrow region near the eutectic component, which makes the aluminate glass less stable and easy to crystallize. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcomings of the current prior art and provide an aluminate glass which is not easy to crystallize, is resistant to thermal shock, is resistant to corrosion, has high hardness, has high infrared transmittance, and is suitable for preparing infrared-transmitting optical devices, and a preparation method thereof.

[0007] The present invention also provides an application of aluminate glass, which has the advantages of high transmittance in the mid-infrared band range of 1μm to 5μm wavelength, high heat shock resistance, high hardness and excellent chemical stability. It is suitable for processing and molding of complex-shaped shapes, and can be used for infrared-transmitting covers, optical windows, infrared night vision devices, infrared spectrometers, optical instruments that require high visible light-infrared transmittance, missile infrared guidance fairings, pods, infrared detectors, infrared cameras, fire warning sensors, infrared camera lenses, etc.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is:

[0009] An aluminate glass, comprising the following components in percentage by weight:

[0010]

[0011]

[0012] Furthermore, an aluminate glass is characterized in that it is preferably composed of the following components in percentage by weight:

[0013]

[0014] Further, an aluminate glass is characterized in that it is preferably composed of the following components in percentage by weight:

[0015]

[0016]

[0017] An aluminate glass characterized by substantially no SiO 2 and B 2 O 3 ;

[0018] An aluminate glass characterized by being substantially free of [OH]- ions, or even if it contains them, they are introduced as impurities from the raw materials or during the preparation process, and the hydroxyl content in the glass is strictly controlled;

[0019] An aluminate glass characterized by substantially not containing oxides of variable valence elements, metal oxides harmful to the environment, and oxides having glass coloring function such as As 2 O 3 , Sb2 O 5 、PbO、CdO、Cr 2 O 3 , CuO, Fe 2 O 3 、CoO、NiO、BeO、CeO 2 、V 2 O 5 , WO 3 、MoO 3 、MnO 2 SnO 2 、Ag 2 O、Nd 2 O 3 Any of the above;

[0020] An aluminate glass, characterized in that the aluminate glass has excellent anti-crystallization performance, heat shock resistance and erosion resistance, and has the characteristics of high hardness and low cost; when the thickness of the aluminate glass is 2.0 mm, its transmittance in the wavelength range of 1 μm to 5 μm is more than 80%; the aluminate glass has good processing performance for a cover with a complex shape, is suitable for processing a complex shape, and can be used to manufacture an infrared-transmitting cover or a round cover;

[0021] Aluminate glass, characterized in that the aluminate glass has excellent chemical stability and a suitable thermal expansion coefficient, a high softening point temperature, good thermal shock resistance, high hardness, and is not easy to crack.

[0022] The present invention also provides a method for preparing aluminate glass, which is characterized by comprising the following steps:

[0023] (1) Glass batching: Before batching, the glass raw materials are subjected to high temperature burning and dehydration treatment at 610-700℃ for 12-23 hours. Water vapor is the main component of gas in glass, which is [OH] - exists in the glass in the form of CO, which has an absorption band at 2.9 μm, while another gas in the glass, CO 2 The absorption band at 2.7μm is strictly controlled. The moisture and hydroxyl content of the raw materials are then proportioned according to the designed components. The corresponding raw material weight is converted according to the weight percentage of each component. Then, each raw material is weighed. Among them, Al 2 O 3 It is introduced by alumina powder, not aluminum hydroxide, and CaO is introduced by Ca(NO 3 ) 2 Introduction;

[0024] (2) Glass melting: Grind and mix the glass batch materials to form a mixture, put the mixture into a platinum crucible, and then put it into a glass melting furnace at 1460℃-1600℃ and heat it for 4 to 8 hours; the glass mixture is melted by atmosphere protection. During the process, water is first removed from the glass melt, and dry argon is blown into the glass melt using a platinum tube to eliminate the hydroxide ions therein. The argon blowing flow rate is 35-49L / min, and dry argon is passed on the surface of the glass melt to prevent reaction with water, thereby improving the transmittance of the glass in the infrared region of the spectrum; since the density of various raw materials varies greatly, it is easy to produce uneven concentration and reduce the transmittance of the glass. Therefore, the glass melt needs to be stirred several times during the melting process to make the glass melt uniform; and the glass melting temperature cannot be too high, which will increase the platinum ions dissolved in the platinum crucible, causing the glass to be colored and the transmittance to decrease;

[0025] (3) Rapid cooling: After the glass is evenly melted, the molten glass is poured into a preheated heat-resistant steel mold and cast into the specified specifications. It is then placed in an annealing furnace for annealing at a temperature of 650-670°C for 6-10 hours. It is then cooled to room temperature in the furnace. Aluminate glass material is obtained by cooling.

[0026] The preparation method of the invention is simple, environmentally friendly and pollution-free, and no heavy metal ions are introduced. The prepared aluminate glass material has excellent infrared transmittance, high hardness, and low cost, and is suitable for body processing and molding preparation with complex shapes. The material can be used for infrared transmittance covers, optical windows, infrared night vision devices, infrared spectrometers, optical instruments requiring high visible light-infrared transmittance, missile infrared guidance fairings, pods, infrared detectors, infrared cameras, fire warning sensors, infrared camera lenses, and the like, and has broad market application prospects.

[0027] Compared with the prior art, the aluminate glass of the present invention has the following characteristics:

[0028] (1) Good anti-crystallization performance;

[0029] (2) Excellent infrared performance, high infrared wavelength transmittance (thickness 2mm, transmittance greater than 80% in the wavelength range of 1μm to 5μm);

[0030] (3) The softening temperature is greater than 750°C and the thermal shock resistance is good;

[0031] (4) Excellent chemical stability;

[0032] (5) Good processing performance of complex-shaped covers;

[0033] (6) It is suitable for the preparation of large-size infrared optical devices, which broadens the application range of aluminate glass.

[0034] The present invention also provides an application of aluminate glass, which has high transmittance in the mid-infrared band within the wavelength range of 1μm to 5μm, and the infrared transmittance of 2.0mm thick glass within the wavelength range of 1μm to 5μm is greater than 80%. It also has the advantages of excellent heat shock resistance and corrosion resistance, high hardness and excellent chemical stability. It is suitable for processing and molding of bodies with complex shapes, and can be used for infrared-transmitting covers, optical windows, infrared night vision devices, infrared spectrometers, optical instruments requiring high visible light-infrared transmittance, missile infrared guidance fairings, pods, infrared detectors, infrared cameras, fire warning sensors, infrared camera lenses, etc.

[0035] In the present invention, Al 2 O 3 It is an intermediate oxide of glass and its content cannot be too small. 2 O 3 It is introduced by alumina powder instead of aluminum hydroxide. The chemical bond strength of Al-O is smaller, which is conducive to the transmission of infrared wavelengths. 3+ When combined with alkaline earth metal oxides, they can capture free oxygen to form [AlO 4 ] uniform network, which reduces the number of broken networks in the glass and is beneficial to reducing crystallization; Al 2 O 3 The weight percentage is 38-45%, Al 2 O 3 The content of Al is lower than 38wt.%, which will reduce the chemical stability of the glass. 2 O 3 The content of is higher than 45wt.%, which will increase the crystallization tendency of the glass.

[0036] Na 2 O is an oxide outside the glass structure network, which can increase the melting performance of the glass. 2 The weight percentage of O is 0.1-1%, Na 2 When the content of O is greater than 1%, the chemical resistance of the glass will be reduced.

[0037] CaO is an external oxide of the glass structure network, and the weight percentage of CaO is 36-43%. If the CaO content is lower than 36wt.%, the glass forming ability will be reduced, and it will be difficult to obtain glass with high infrared transmittance. If the CaO content is higher than 43wt.%, the chemical resistance of the glass will be reduced, and the crystallization tendency of the glass will be increased.

[0038] MgO is a network oxide of glass structure, and is a member of the same family as Ca. The properties and functions of the two are similar in glass. The introduction of network oxides with similar properties in the same valence into glass can improve the performance of glass. The number of ions in glass increases, and they interfere with each other during the crystallization process, which can reduce the crystallization rate and make the glass stable. The weight percentage of MgO is 0.1-1%. If the content of MgO is less than 0.1wt.%, the chemical stability of glass will be reduced. If the content of MgO is greater than 1wt.%, the tendency of glass to crystallize will be increased.

[0039] SrO is also a network exometallic oxide of the glass structure. It is a member of the same family as Ca. The properties and functions of the two are similar in glass. The introduction of network exometallic oxides with similar properties in the same valence into the glass can improve the performance of the glass. The number of ions in the glass increases, and they interfere with each other during the crystallization process, which can reduce the crystallization rate and make the glass stable. The weight percentage of SrO is 0.5-3.9%. If the content of SrO is less than 0.5%, the chemical stability of the glass will be reduced. If the content of SrO is greater than 3.9wt.%, the tendency of crystallization of the glass will be increased.

[0040] BaO is an oxide outside the glass structure network. BaO can increase the quality of cations and increase the infrared transmission wavelength range. BaO is composed of Ba(NO 3 ) 2 Introduction; the weight percentage of BaO is 0.5-3.9%. When the content of BaO is less than 0.5%, the infrared transmittance of the glass will be reduced. When the content of BaO is greater than 3.9wt.%, the crystallization temperature of the glass will be increased, the crystallization tendency of the glass will be increased, and the density of the glass will be significantly improved.

[0041] G 2 O 3 It is a rare earth oxide, Gd 3+ The large ion radius and strong electric field produce a strong aggregation effect in the glass, which can increase the quality of cations, increase the infrared transmission wavelength range, and improve the chemical stability of the glass. 2 O 3 The weight percentage is 1-10%, Gd 2 O 3 The content of Gd is less than 1%, which will reduce the infrared transmittance of the glass. 2 O 3 When the content is greater than 10 wt.%, the density and thermal expansion coefficient of the glass will increase, and the softening point temperature of the glass will decrease.

[0042] GeO 2It is a glass-forming oxide that can improve the performance of glass with high infrared transmittance in the wavelength range of 1μm to 5μm. The chemical bond strength of Ge-O is weaker than that of Si-O and BO, the attraction between ions is small, and the infrared transmission wavelength is farther; GeO 2 The weight percentage is 0.5-5%, GeO 2 When the content is lower than 0.5wt.%, it is difficult to obtain glass with high infrared transmittance, and the chemical resistance of the glass will be reduced. 2 When the content is higher than 5 wt.%, the hardness of the glass will be reduced and the phase separation tendency of the glass will be increased.

[0043] ZrO 2 The introduction of ZrO is to enhance the hardness of glass. 2 The weight percentage is 0.1-1%, ZrO 2 The introduction amount of more than 1% will make the glass difficult to melt, and at the same time it will reduce the transmittance of the glass and increase the crystallization tendency of the glass.

[0044] The introduction of ZnO is to improve the melting performance of glass and is used as a flux. 2 O 3 The use of ZnO can effectively improve the chemical stability and infrared transmittance of the glass; the weight percentage of ZnO is 0.5-4.9%, and the introduction amount of ZnO greater than 4.9% will reduce the transmittance of the glass and increase the crystallization tendency of the glass.

[0045] Ga 2 O 3 It can increase the quality of cations. Due to its ultra-wideband spectroscopy characteristics in the infrared band, it can increase the infrared transmission wavelength range. 2 O 3 The weight percentage is 0.1-1%, Ga 2 O 3 The content of Ga is less than 0.1%, which will reduce the infrared transmittance of the glass. 2 O 3 If the content is greater than 1%, the chemical resistance of the glass will be reduced.

[0046] TiO 2 It is used to lower the crystallization temperature of glass. 4+ When combined with alkaline earth metal oxides, they can capture free oxygen to form [TiO 4 ] uniform network, which reduces the number of broken networks in the glass and is beneficial to reducing crystallization; TiO 2 The weight percentage is 0.1-2.5%, TiO 2 If the content is greater than 2.5wt.%, the infrared transmittance of the glass will be reduced.

[0047] The aluminate glass of the present invention substantially does not contain glass network former oxide SiO 2 and B 2 O 3 ; It does not contain [OH] - ; It does not contain oxides of variable valence elements, metal oxides that are harmful to the environment, and oxides with glass coloring functions such as As 2 O 3 , Sb 2 O 5 、PbO、CdO、Cr 2 O 3 , CuO, Fe 2 O 3 、CoO、NiO、BeO、CeO 2 、V 2 O 5 , WO 3 、MoO 3 、MnO 2 SnO 2 、Ag 2 O、Nd 2 O 3 Any of the above; substantially free of specific components here means that they are not intentionally added, and does not exclude extremely small amounts of impurities inevitably mixed in from raw material impurities, etc., which will not affect the desired properties. Even if extremely small amounts are contained, they are brought in by other glass raw materials. However, when introducing these variable valence elements into the glass raw materials, the content must be strictly controlled below 1ppm.

[0048] The present invention successfully prepares an aluminate glass material with heat shock resistance, corrosion resistance, high hardness, low cost and high infrared transmittance. The aluminate glass has high transmittance in the mid-infrared band range of 1μm to 5μm wavelength, and the infrared transmittance of 2.0mm thick glass in the wavelength range of 1μm to 5μm is greater than 80%. It also has the advantages of excellent heat shock resistance, corrosion resistance, high hardness and excellent chemical stability, and is suitable for complex shape processing and molding preparation.

[0049] The present invention also provides an application of aluminate glass, which can be used in infrared-transmitting covers, optical windows, infrared night vision devices, infrared spectrometers, optical instruments requiring high visible light and infrared transmittance, missile infrared guidance fairings, pods, infrared detectors, infrared cameras, fire warning sensors, infrared camera lenses, etc. DETAILED DESCRIPTION

[0050] In order to make the purpose, technical scheme and advantages of the present invention clearer, the following is a further detailed description of the embodiments of the present invention. Table 1 lists in detail the glass chemical composition (wt.%) and glass transmittance performance of the embodiment. Among them, the infrared light transmittance spectrum is tested when the sample thickness is 2mm after surface grinding and polishing according to the test requirements, and the infrared band range of the test is 1μm~5μm infrared light transmittance. The detection instruments use Varian Cary-50 spectrophotometer and Varian Scimitar-1000 Fourier transform infrared spectrometer.

[0051] In addition, the water resistance stability of aluminate glass was tested with reference to the method of GB / T 12416.2-1990 "Test method and classification of water resistance of glass particles at 121°C", and the softening temperature was tested with reference to the method of GB / T 7962.16-2010 "Test method for colorless optical glass Part 16: Linear expansion coefficient, transition temperature and sag temperature".

[0052] Table 1 Chemical composition (wt.%) and glass properties of the examples

[0053]

[0054] Example 1

[0055] First, glass raw materials are selected according to the glass composition of Example 1 in Table 1. The raw materials are required to be aluminum oxide powder (analytical grade, 150 μm sieve material is less than 1%, 45 μm sieve material is less than 30%), sodium carbonate (analytical grade), calcium nitrate (analytical grade, average particle size 250 μm), magnesium oxide (analytical grade), strontium carbonate (analytical grade), barium nitrate (analytical grade), gadolinium oxide (5N), germanium oxide (analytical grade), zirconium oxide (analytical grade), zinc oxide (analytical grade), gallium oxide (5N), and titanium oxide (analytical grade). The main raw materials in the glass raw materials are subjected to high-temperature calcination dehydration treatment at 610° C. for 23 hours to reduce the moisture and hydroxyl content of the glass raw materials, and the moisture and hydroxyl content of the raw materials are strictly controlled. Then the high-purity raw materials are mixed according to the glass chemical composition of Table 1. The mixture was weighed, and then the raw materials were ground and mixed to form a mixture. The mixture was placed in a platinum crucible and then placed in a glass melting furnace at 1600°C for heating for 4 hours. When the glass mixture was melted, atmosphere protection was used for melting. Argon was blown into the glass melt using a platinum tube. Dry argon was introduced into the surface of the glass melt to prevent reaction with water. The flow rate of argon blowing was 49L / min. During the glass melting process, the glass melt was stirred 2 to 3 times to make it uniform. After the glass was melted uniformly, the molten glass was poured into a preheated heat-resistant steel mold and cast into the specified test sample requirements. Then, the glass was placed in an annealing furnace for annealing at a temperature of 670°C and a annealing time of 6 hours. The aluminate glass material was obtained by cooling the furnace. Its test properties are shown in Table 1.

[0056] Example 2

[0057] The actual composition of the glass is shown in Table 1 in Example 2. The same raw materials as in Example 1 are used, and the raw materials are subjected to a high temperature burning and dehydration treatment of 700°C for 12 hours, and a melting process of melting at 1460°C for 8 hours. Argon gas is blown into the glass melt using a platinum tube, and dry argon gas is introduced on the surface of the glass melt to prevent reaction with water. The flow rate of argon gas blowing is 35L / min. After the glass melts uniformly, the molten glass is poured into a preheated heat-resistant steel mold and cast into the specified test sample requirements, and then placed in an annealing furnace for annealing treatment. The annealing temperature is 650°C, the annealing time is 10 hours, and the aluminate glass material is obtained by cooling in the furnace. The same test conditions as in Example 1 are adopted, and the basic properties of the sample are shown in Table 1.

[0058] Example 3

[0059] The actual composition of the glass refers to Example 3 in Table 1, using the same raw materials and raw material requirements as Example 1, and adopting a melting process system and annealing process system of melting at 1560°C for 6 hours and the same test conditions as Example 1. The basic properties of the sample are shown in Table 1.

[0060] Example 4

[0061] The actual composition of the glass refers to Example 4 in Table 1, using the same raw materials and raw material requirements as Example 1, and adopting the same melting process system, annealing process system and test conditions. The basic properties of the sample are shown in Table 1.

[0062] Example 5

[0063] The actual composition of the glass refers to Example 5 in Table 1, using the same raw materials and raw material requirements as Example 1, and adopting the same melting process system, annealing process system and test conditions. The basic properties of the sample are shown in Table 1.

[0064] The present invention successfully prepares an aluminate glass material with heat shock resistance, corrosion resistance, high hardness, low cost and high infrared transmittance. The aluminate glass has the advantages of greater than 80% infrared light transmittance in the mid-infrared band range of 1μm to 5μm when the thickness is 2mm, high heat shock resistance, high hardness and excellent chemical stability, and is suitable for body processing and molding preparation with complex shapes, and can be used for infrared-transmitting covers, optical windows, infrared night vision devices, infrared spectrometers, optical instruments requiring high visible light-infrared transmittance, missile infrared guidance fairings, pods, infrared detectors, infrared cameras, fire warning sensors, infrared camera lenses, etc.

[0065] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. An aluminate glass, characterized in that: The following components are contained in percentage by weight composition:

2. The aluminate glass according to claim 1, characterized in that: Preferably, the following weight percentage components are used: composition:

3. An aluminate glass according to claim 1 or claim 2, characterized in that: Preferably, the following weight percentage components are used: composition:

4. The aluminate glass according to claim 1, characterized in that: Contains virtually no [OH] - Ions, even if they are present, are brought in as impurities from the raw materials or during the preparation process. The hydroxyl content in the glass must be strictly controlled.

5. The aluminate glass according to claim 1, characterized in that: It does not contain substantially any of As2O3, Sb2O5, PbO, CdO, Cr2O3, CuO, Fe2O3, CoO, NiO, BeO, CeO2, V2O5, WO3, MoO3, MnO2, SnO2, Ag2O, and Nd2O3.

6. The aluminate glass according to claim 1, characterized in that: When the thickness of the aluminate glass is 2.0 mm, its transmittance in the wavelength range of 1 μm to 5 μm is above 80%.

7. The method for preparing aluminate glass according to claim 1, characterized in that: The following steps are involved: (1) Glass batching: Before batching, the glass raw materials are subjected to high-temperature burning and dehydration treatment at 610-700°C for 12-23 hours, and the moisture and hydroxyl content of the raw materials are strictly controlled. Then, the high-purity raw materials are proportioned according to the designed components, and the corresponding raw material weight is converted according to the weight percentage of each component. Then, each raw material is weighed, wherein Al2O3 is introduced by alumina powder, and aluminum hydroxide is not used for introduction, and CaO is introduced by Ca(NO3)2; (2) Glass melting: Grind and mix the glass batch materials to form a mixture, put the mixture into a platinum crucible, and then put it into a glass melting furnace at 1460°C-1600°C for heating for 4 to 8 hours; when the glass mixture is melted, atmosphere protection is adopted, and dry argon gas is blown into the glass melt through a platinum tube to eliminate the hydroxide therein, and the flow rate of argon gas blown is 35-49L / min, and dry argon gas is passed on the surface of the glass melt to prevent reaction with water, so as to improve the transmittance of the glass in the infrared region of the spectrum; during the melting process, the glass melt needs to be stirred several times to make the glass melt uniform; (3) Rapid cooling: After the glass is evenly melted, the molten glass is poured into a preheated heat-resistant steel mold and cast into the specified specifications. It is then placed in an annealing furnace for annealing at a temperature of 650-670°C for 6-10 hours. It is then cooled to room temperature in the furnace. Aluminate glass material is obtained by cooling.

8. An application of aluminate glass prepared by the method for preparing aluminate glass according to claim 7, characterized in that: The aluminate glass can be used for infrared-transmitting covers, optical windows, infrared night vision devices, infrared spectrometers, optical instruments requiring high visible light and infrared transmittance, missile infrared guidance fairings, pods, infrared detectors, infrared cameras, fire warning sensors, and infrared camera lenses.

Citation Information

Patent Citations

  • Aluminate glass, preparation thereof and application thereof

    CN102584011A

  • Infrared-permeable calcium aluminate glass preparation method

    CN105198209A

  • Infrared-transmitting glass

    CN106573824A

  • Optical glass, preform, and optical element and optical device

    CN107879619A

  • Germanate infrared transmitting glass and preparation method thereof

    CN110194591A