A method for activating coal gangue and cement

By spraying metal salt solution and covering the modified slurry during the calcination process, the activity and color of coal gangue are improved, and the problem of limited application of coal gangue in the cement industry is solved, achieving high proportional addition and cost reduction Effect.

CN116395995BActive Publication Date: 2024-11-01YAOBAI SPECIAL CEMENT TECH R&D CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310154479.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-22
Publication Date
2024-11-01
Estimated Expiration
2043-02-22

AI Technical Summary

Technical Problem

The application of coal gangue in the cement industry is limited by its color changes and low activity, which leads to limited incorporation and inability to effectively utilize a large amount of coal gangue resources.

Method used

By calcining coal gangue in an oxidation atmosphere of 600-900°C, spraying metal salt solution and covering modified semi-activated coal gangue slurry during cooling, it stimulates its activity, changes color and increases activity, so that it can be used in high-quality The proportions are added to the cement.

Benefits of technology

The color of calcined coal gangue has been successfully changed, making its activity reaching 80-93%. More than 30% can be added to cement without changing the color, which reduces the cost of cement and improves the activity of coal gangue. It is suitable for cement and wall materials. and other industries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004091802620000011
    Figure HDA0004091802620000011
Patent Text Reader

Abstract

The present invention relates to a coal gangue treatment technology, and in particular to a coal gangue activation method and related cement. The method comprises calcining a first coal gangue at 600-900°C in an oxidizing atmosphere, cooling it, spraying a room-temperature metal salt solution on the surface of the coal gangue during the cooling process; after spraying, covering the surface of the coal gangue with a room-temperature modified semi-activated coal gangue slurry, and then cooling it until the material as a whole drops to room temperature; the preparation method of the modified semi-activated coal gangue slurry comprises: calcining and crushing a second coal gangue at 600-700°C in an oxidizing atmosphere to obtain a semi-activated coal gangue powder, and then soaking the semi-activated coal gangue powder in a C2H2O4 solution to obtain a modified semi-activated coal gangue slurry. The present invention can change the color of the calcined coal gangue, make the activated coal gangue brown, and its activity reaches 80-93%, and can be used as a cement admixture, with a large addition amount and a normal cement color.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coal gangue treatment, and in particular to a coal gangue activation method and related cement. Background Art

[0002] Gangue is solid waste removed during coal mining and washing. my country is a major coal producer, and the amount of gangue emissions is huge, accounting for about 10-20% of coal production. By 2022, the cumulative stockpile of gangue in my country will exceed 7 billion tons, and the amount will increase by 100 million tons each year. Large-scale disposal and high-value comprehensive utilization of gangue are severe challenges facing my country.

[0003] Calcined coal gangue is used as a cement mixing material, which is an effective way to utilize coal gangue. However, after calcined (including spontaneous combustion) coal gangue, its color is red. When the amount of cement mixed in is greater than 5%, the color of the cement turns red, which is not accepted by users. In addition, due to its low activity, when producing cement with the production number (PC42.5), the mixing amount is very small (≤10%), which seriously restricts the resource utilization of coal gangue in the cement industry. Summary of the invention

[0004] In view of the defects or shortcomings of the prior art, the present invention provides a method for activating coal gangue. To this end, the method provided by the present invention comprises:

[0005] The first coal gangue is calcined at 600-900°C in an oxidizing atmosphere, and then cooled. During the cooling process, a room-temperature metal salt solution is sprayed on the surface of the coal gangue; after the spraying, the room-temperature modified semi-activated coal gangue slurry is covered on the surface of the coal gangue, and then cooled until the entire material drops to room temperature;

[0006] The metal salt is selected from one of copper salts, indium salts, alkali metal salts and alkaline earth metal salts, or a mixture of two or more metal salts;

[0007] The preparation method of the modified semi-activated coal gangue slurry comprises: calcining and crushing the second coal gangue at 600-700° C. in an oxidizing atmosphere to obtain semi-activated coal gangue powder, and then soaking the semi-activated coal gangue powder in a C2H2O4 solution to obtain modified semi-activated coal gangue slurry.

[0008] An optional solution is that the particle size of the first coal gangue is ≤50mm.

[0009] An optional solution is to calcine the first coal gangue at 600-900° C. in an oxidizing atmosphere for 3-6 hours.

[0010] An optional solution is that the mass percentage concentration of the metal salt solution is 1% to 3%.

[0011] An optional solution is that the particle size of the second coal gangue is ≤50mm.

[0012] An optional solution is that the particle size of the semi-activated coal gangue powder is ≤2mm.

[0013] An optional solution is to calcine the second coal gangue at 600-700° C. in an oxidizing atmosphere for 0.5-1.0 h.

[0014] An optional solution is to soak the semi-activated coal gangue powder in a C2H2O4 solution for 3 to 5 hours.

[0015] An optional solution is that the mass ratio of the first coal gangue, the metal salt, the second coal gangue, and C2H2O4 is: 10-20:1-3:3-5:1-3.

[0016] An optional solution is that the mass percentage concentration of the C2H2O4 solution is 10% to 20%.

[0017] An optional solution is that the first coal gangue and the second coal gangue have the same or different sources.

[0018] An optional solution is that the semi-activated coal gangue powder has a covering thickness of 30 to 50 mm.

[0019] Alternatively, the mixture may be cooled to room temperature and then crushed.

[0020] An optional solution is that the cooling is natural cooling after stopping heating.

[0021] The present invention also provides corresponding cement, wherein the activated coal gangue is added to the cement. An optional solution is that the amount of coal gangue added to the cement is 5% to 30%.

[0022] The present invention can change the color of calcined (including spontaneous combustion) coal gangue and make the activated coal gangue brown. The activity of the activated coal gangue reaches 80-93% (GB / T1596-2017). The activated coal gangue can be used as a cement admixture with a large addition amount (the addition amount can reach 30%) and the cement has a normal color. The activated coal gangue is suitable for industries such as cement and wall materials.

[0023] The gangue activation and color adjustment technology of the present invention is suitable for calcining gangue in any kiln. The calcination temperature of gangue is relatively low. The type of gangue can be gangue containing spontaneous combustion. The calcined gangue is only treated with a modifier, and the method is simple. Due to the simple treatment method, the treatment cost per ton of gangue is only a dozen yuan, which will greatly reduce the cost of cement. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The products obtained in the examples and comparative examples of the present invention, wherein (a) is the product obtained in Example 1 (brown); (b) is the product obtained in Comparative Example 2 (yellow); and (c) is the product obtained in Comparative Example 1 (yellowish brown). DETAILED DESCRIPTION

[0025] Unless otherwise specified, the scientific and technical terms used herein are understood according to the knowledge of ordinary technicians in the relevant fields.

[0026] The present invention first places the coal gangue in a kiln and calcines it at 600-900°C in an oxidizing atmosphere. After the coal gangue is calcined, on the one hand, carbon and organic matter therein are burned to generate carbon dioxide and emit it, so that the loss on ignition is reduced. On the other hand, minerals such as clay are dehydrated and decomposed to form amorphous metakaolin and silicon dioxide (SIO2) and aluminum oxide (Al2O3) with high activity. The high-temperature coal gangue is in an oxidizing atmosphere, and the color of the coal gangue changes from black gray to light red.

[0027] During the cooling process of the calcined gangue, a metal salt solution is sprayed on the surface to modify the hot gangue. When the water in the metal salt solution meets the hot gangue, it quickly absorbs heat and vaporizes, causing the gangue to cool rapidly, further retaining the activity of amorphous metakaolin and silicon dioxide (SIO2) and aluminum oxide (Al2O3) produced by the high-temperature thermal activation of the gangue; at the same time, the metal salt further stimulates the intrinsic activity of the calcined gangue.

[0028] Under the catalysis of metal salt ions, CO, H2, and H2O, the dark red ferric oxide (Fe2O3) and elemental iron (Fe) in the gangue are reduced to form black ferroferric oxide (Fe3O4), which makes the red gangue at high temperature turn into brown gangue and the brown gangue is retained after rapid cooling;

[0029] The calcined coal gangue is subjected to secondary treatment of modified slurry and rapid cooling to retain highly active amorphous kaolin, silicon dioxide (SIO2) and aluminum oxide (Al2O3), and the coal gangue is further activated multiple times.

[0030] The activated gangue of the present invention is added to cement. When the cement is hydrated, the activity of sulfate ions is greatly improved under the catalytic system of metal salt ions. Sodium sulfate can react with calcium hydroxide precipitated by cement hydration to accelerate the hydration of tricalcium silicate, so that C3A in cement reacts with SO4 2- The hydration reaction of calcium hydroxide to form calcium sulfoaluminate is accelerated, and the calcium hydroxide released by C3S hydration is consumed, so that the hydration of C3S is accelerated. At the same time, the active components of silicon dioxide (SIO2) and aluminum oxide (Al2O3) in coal gangue are stimulated to form the dominant strength product calcium silicate hydrate and the drought strength products calcium sulfoaluminate hydrate and calcium aluminate hydrate.

[0031] The following are specific examples provided by the inventors to further explain the present invention. It should be noted that the temperature, concentration, and duration involved in this article are approximate values ​​for illustrative purposes. In the specific scheme, the skilled person can select the material ratio, concentration, and temperature involved in the method according to the content disclosed in the present invention using a conventional experimental period to achieve the purpose of the present invention.

[0032] The method for detecting the activity of coal gangue in the following embodiments refers to GB / T1596-2017, and is specifically calculated using the following formula:

[0033] H28=R28 gangue / R28 cement*100%

[0034] Where:

[0035] H28: Test sample intensity activity index;

[0036] R28 gangue: 28-day compressive strength of activated coal gangue mortar (MPa);

[0037] R28 cement: PO42.5 cement mortar 28-day compressive strength (MPa);

[0038] Among them, the activated coal gangue mortar is made into 160x40x40mm test blocks with the ratio of PO42.5 cement: activated coal gangue = 70:30 (according to GB / T17671-2021) and put into the water pool for curing. The ratio of its 28-day mortar strength and the 28-day compressive strength of PO42.5 cement mortar is measured and multiplied by 100 as its activity index.

[0039] The first coal gangue and the second coal gangue used in the following examples have the same source, and their main chemical compositions are: SIO2: 53.48%, AI203: 15.22%, Fe2O3: 6.07%, CaO: 2.56%, MgO: 1.59%, SO3: 0.49%, K20: 0.7%, Na2O: 1.0%, LOSS: 15.62%, and are black in color.

[0040] Cement: PO42.5.

[0041] Embodiment 1:

[0042] In this embodiment, the mass ratio of the first coal gangue, the metal salt, the second coal gangue, and C2H2O4 is 20:1:3:1.

[0043] The first coal gangue with a particle size of ≤50 mm was calcined at 900°C for 3 hours and then naturally cooled;

[0044] During the natural cooling process, a Ca(NO3)2 aqueous solution with a mass percentage concentration of 2% is first sprayed on the surface of the coal gangue;

[0045] After spraying, the modified semi-activated coal gangue slurry is covered on the surface of the coal gangue, and the covering thickness is 40mm; the preparation method of the modified semi-activated coal gangue slurry in this embodiment is: the second coal gangue with a particle size of ≤50mm is calcined at 600℃ for 0.5h, and crushed to form semi-activated coal gangue powder of <2mm; then the semi-activated coal gangue powder is soaked in a C2H2O4 solution with a mass percentage concentration of 10%, and the overall slurry after soaking for 3h is the modified semi-activated coal gangue slurry obtained;

[0046] Then the whole material is cooled to room temperature and then crushed to activate the coal gangue material to a specific gravity of 500-600m 2 / kg.

[0047] The activated coal gangue obtained in this embodiment is brown in color (such as Figure 1 a);

[0048] After adding 30% of the coal gangue of this embodiment to PO42.5 cement, the color of the cement did not change;

[0049] After testing, the 28-day compressive strength (R28 gangue) of the activated coal gangue obtained in this embodiment is 42.4 MPa; and the activity (H28) is 82%.

[0050] Comparative Example 1:

[0051] The difference between this comparative example and Example 1 is that no metal salt solution is sprayed. The color of the obtained coal gangue is: yellowish brown (such as Figure 1 c), the 28-day compressive strength of coal gangue (R28 gangue) is 39.8MPa, and the activity (H28) is 77%. After adding 30% of the coal gangue of this comparative ratio to PO42.5 cement, the color of the cement changes.

[0052] Comparative Example 2:

[0053] The difference between this comparative example and Example 1 is that the modified semi-activated coal gangue slurry is not covered. The color of the obtained coal gangue is yellow (such as Figure 1 As shown in Figure b), the 28-day compressive strength of coal gangue (R28 gangue) is 40.8MPa, and the activity (H28) is 79%. After adding 30% of the coal gangue of this comparative ratio to PO42.5 cement, the color of the cement changes.

[0054] Comparative Example 3:

[0055] The difference between this comparative example and Example 1 is that the modified semi-activated coal gangue slurry is replaced with gasified slag. The color of the obtained coal gangue is yellow-brown, the 28-day compressive strength of the coal gangue (R28 gangue) is 33.1 MPa, and the activity (H28) is 64%. After adding 30% of the coal gangue of this comparative example to PO42.5 cement, the color of the cement changes.

[0056] Comparative Example 4:

[0057] The difference between this comparative example and Example 1 is that the semi-activated coal gangue powder is replaced with gasified slag and lead-zinc ore tailings. The color of the obtained coal gangue is yellow-brown; the 28-day compressive strength of the coal gangue (R28 gangue) is 32MPa, and the activity (H28) is 62%; the activity is greatly reduced. After adding 30% of the coal gangue of this comparative example to PO42.5 cement, the color of the cement changes.

[0058] Embodiment 2:

[0059] This embodiment is different from embodiment 1 in that: the mixture of metal salts CuCl2 and Na2SO4, and the mass ratio of CuCl2:Na2SO4 is 1:1; the mass percentage concentration of the metal salt solution is 1%;

[0060] In this embodiment, the mass ratio of the first coal gangue, the metal salt, the second coal gangue, and C2H2O4 is: 15:1:4:2;

[0061] The first coal gangue calcination temperature is 600℃ and the time is 6h;

[0062] The second gangue calcination temperature is 650℃, and the time is 1h;

[0063] The semi-activated coal gangue powder was immersed in a C2H2O4 solution with a mass percentage concentration of 12% for 5 hours to obtain a modified semi-activated coal gangue slurry;

[0064] The obtained coal gangue is brown in color, and the 28-day compressive strength of the coal gangue (R28 gangue) is 43.1MPa; the activity (H28) is 84%.

[0065] Embodiment 3:

[0066] The difference between this embodiment and embodiment 1 is that the metal salt is Na2SiO3, and the mass percentage concentration of the metal salt is 3%;

[0067] In this embodiment, the mass ratio of the first coal gangue, the metal salt, the second coal gangue, and C2H2O4 is: 10:1:5:3;

[0068] The first coal gangue calcination temperature is 750℃ and the time is 3h;

[0069] The second gangue calcination temperature is 680℃, and the time is 1h;

[0070] The semi-activated coal gangue powder was soaked in a C2H2O4 solution with a mass percentage concentration of 15% for 4 hours.

[0071] The obtained coal gangue is brown in color, and the 28-day compressive strength of the coal gangue (R28 gangue) is 46MPa; the activity (H28) is 89%.

[0072] Embodiment 4:

[0073] This embodiment is different from embodiment 1 in that: the metal salt is a mixture of CuCl2:In2(SO4)3, and the mass ratio of CuCl2:In2(SO4)3 is 1:1; the mass percentage concentration of the metal salt solution is 1.5%;

[0074] In this embodiment, the mass ratio of the first coal gangue, the metal salt, the second coal gangue, and C2H2O4 is: 20:2:5:2;

[0075] The first coal gangue calcination temperature is 850℃, and the time is 5h;

[0076] The semi-activated coal gangue powder was soaked in a C2H2O4 solution with a mass percentage concentration of 15% for 4 h.

[0077] The color of the obtained coal gangue is brown, and the 28-day compressive strength of the coal gangue (R28 gangue) is 46MPa; the activity (H28) is 89%.

[0078] Embodiment 5:

[0079] This embodiment is different from embodiment 1 in that the metal salt is a mixture of CuCl2, In2(SO4)3 and Na2SO4, and the mass ratio of CuCl2:In2(SO4)3:Na2SO4 is 1:0.2:3, and the mass percentage concentration of the metal salt solution is 3%;

[0080] In this embodiment, the mass ratio of the first coal gangue, the metal salt, the second coal gangue, and C2H2O4 is: 20:3:5:3;

[0081] The first coal gangue calcination temperature is 800℃ and the time is 4h;

[0082] The second coal gangue calcination temperature is 700℃, and the time is 1h;

[0083] Semi-activated coal gangue powder was modified by soaking in 18% C2H2O4 solution for 3 h.

[0084] The color of the obtained coal gangue is brown, and the 28-day compressive strength of the coal gangue (R28 gangue) is 47.6MPa; the activity (H28) is 92%.

[0085] Embodiment 6:

[0086] This embodiment is different from embodiment 1 in that the metal salt is a mixture of CuCl2, In2(SO4)3 and Na2SiO3, and the mass ratio of CuCl2:In2(SO4)3:Na2SiO3 is 1:0.2:1, and the mass percentage concentration of the metal salt solution is 3%;

[0087] In this embodiment, the mass ratio of the first coal gangue, the metal salt, the second coal gangue, and C2H2O4 is: 20:3:5:3;

[0088] The first coal gangue calcination temperature is 800℃ and the time is 6h;

[0089] Semi-activated coal gangue powder was modified by soaking in 20% C2H2O4 solution for 3 h.

[0090] The obtained coal gangue is brown in color, with a 28-day compressive strength (R28 gangue) of 48.2 MPa and an activity (H28) of 93.

Claims

1. A method for activating coal gangue, Characterized in that the method include: The first gangue is calcined at 600-900°C in an oxidizing atmosphere, and then cooled. During the cooling process, a room-temperature metal salt solution is sprayed on the surface of the gangue. After the spraying, the surface of the gangue is covered with a room-temperature modified semi-activated gangue slurry, and then cooled until the entire material drops to room temperature. The metal salt is selected from one of copper salts, indium salts, alkali metal salts and alkaline earth metal salts, or a mixture of two or more metal salts; The preparation method of the modified semi-activated coal gangue slurry comprises: calcining and crushing the second coal gangue at 600-700°C in an oxidizing atmosphere to obtain semi-activated coal gangue powder; then soaking the semi-activated coal gangue powder in C 2 H 2 O 4 A modified semi-activated coal gangue slurry is obtained in the solution; First coal gangue, metal salt, second coal gangue, C 2 H 2 O 4 The mass ratio is: 10~20:1~3:3~5:1~3.

2. The method for activating coal gangue according to claim 1, It is characterized in that The particle size of the first coal gangue is ≤50mm.

3. The method for activating coal gangue according to claim 1, It is characterized in that The first coal gangue is calcined at 600-900° C. in an oxidizing atmosphere for 3-6 hours.

4. The method for activating coal gangue according to claim 1, It is characterized in that The mass percentage concentration of the metal salt solution is 1% to 3%.

5. The method for activating coal gangue according to claim 1, It is characterized in that The particle size of the second coal gangue is ≤50mm.

6. The method for activating coal gangue according to claim 1, It is characterized in that The particle size of semi-activated coal gangue powder is ≤2mm.

7. The method for activating coal gangue according to claim 1, It is characterized in that The second coal gangue is calcined at 600-700° C. in an oxidizing atmosphere for 0.5-1.0 h.

8. The method for activating coal gangue according to claim 1, It is characterized in that Semi-activated coal gangue powder in C 2 H 2 O 4 The soaking time in the solution is 3 to 5 hours.

9. The method for activating coal gangue according to claim 1, It is characterized in that The C 2 H 2 O 4 The mass percentage concentration of the solution is 10% to 20%.

10. The method for activating coal gangue according to claim 1, It is characterized in that The first coal gangue and the second coal gangue may have the same or different sources.

11. The method for activating coal gangue according to claim 1, It is characterized in that The covering thickness of the modified semi-activated coal gangue powder is 30 to 50 mm.

12. The method for activating coal gangue according to claim 1, It is characterized in that Cool to room temperature and then crush.

13. The method for activating coal gangue according to claim 1, It is characterized in that The cooling is natural cooling after stopping heating.

14. A cement, It is characterized in that The cement is added with coal gangue activated by the method according to any one of claims 1 to 13.

15. The cement according to claim 14, It is characterized in that The coal gangue is added in an amount of 5% to 30% in cement.