Hydrogenation catalyst and preparation method thereof, method and system for producing solvent oil by reforming raffinate oil

Through the combined use of high nickel content hydrogenation catalysts and molecular sieve adsorbents, the problems of low utilization rate and short catalyst life in reforming raffinate treatment are solved, efficient production of high-purity solvent oil is achieved, and the start-up process of the device is simplified and reduced. cost.

CN116408090BActive Publication Date: 2024-10-15PETROCHINA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111674373.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-31
Publication Date
2024-10-15
Estimated Expiration
2041-12-31

AI Technical Summary

Technical Problem

The existing reforming raffinate treatment technology has problems such as low utilization rate, single processed product, low product yield, and short hydrogenation catalyst operation cycle. Especially when the benzene and olefin content is high, it is difficult to meet the requirements of high-purity solvent oil. Production needs, and the pre-sulfidation of hydrodesulfurization catalysts and the pre-reduction of high-nickel catalysts are cumbersome, affecting the start-up cycle of the device.

Method used

A hydrogenation catalyst with a high nickel content is used, which is composed of a carrier and a loaded first active metal component and a second active metal component to improve the dispersion of nickel and the hydrogenation active center, and is combined with a molecular sieve adsorbent for desulfurization and dehydration Treatment, using a hydrogenation catalyst to carry out hydrogenation and debenzenization and deolefinization reactions, and improving the purity and yield of solvent oil through distillation and normalization reactions.

Benefits of technology

It effectively increases the added value of reforming raffinate, extends the service life of hydrogenation catalysts, reduces operating costs, and enables efficient use of reforming raffinate to produce a variety of high-purity solvent oils that meet the requirements for benzene content and bromine index. Standard requirements and simplify the installation start-up process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116408090B_ABST
    Figure CN116408090B_ABST
Patent Text Reader

Abstract

The present invention provides a hydrogenation catalyst and a preparation method thereof, a method and system for producing solvent oil from reformed raffinate oil. The hydrogenation catalyst comprises a carrier, a first active metal component, and a second active metal component, wherein the first active metal component comprises nickel, and the weight content of the first active metal component in the catalyst is 40-70%. The present invention also provides a preparation method for the above-mentioned catalyst. The present invention provides a method for producing solvent oil from reformed raffinate oil, which utilizes the above-mentioned catalyst to perform hydrogenation debenzenization and deolefination reactions on the reformed raffinate oil after desulfurization and dehydration. The present invention also provides a system for producing solvent oil from reformed raffinate oil that can implement the above-mentioned method. The method is suitable for the separation and utilization of reformed raffinate oil with high benzene and olefin content, and can utilize reformed raffinate oil to produce a variety of solvent oils, effectively improving the added value of reformed raffinate oil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of reforming raffinate oil processing, and in particular to a hydrogenation catalyst and a preparation method thereof, and a method and system for producing solvent oil from reforming raffinate oil. Background Art

[0002] Reforming raffinate is a by-product of aromatics production. It is a good petrochemical raw material due to its low content of impurities such as sulfur, nitrogen and heavy metals. Different high value-added components can be distilled according to different boiling points. It is suitable for the production of high-quality solvent oil and high value-added hexane oil and isohexane oil.

[0003] Reforming raffinate contains a small amount of unsaturated components such as olefins and aromatics, which seriously affect the properties of raffinate as a high-value-added solvent oil. For example, n-hexane is mainly used as a solvent for the polymerization of olefins such as propylene, an extractant for edible vegetable oils, a solvent for rubber and paints, and a pigment diluent, etc., and there are clear restrictions on unsaturated hydrocarbons such as benzene; 6# solvent oil is an organic solvent used to produce edible oils and fats. Some residues will remain in the edible oils and fats during the production process, and the carcinogen aromatic hydrocarbons in the solvent oil will also remain in the edible oils and fats, causing harm to the human body. The aromatic hydrocarbon content in 6# solvent oil must be strictly controlled; pentane foaming agent is mainly used as a solvent, to make artificial ice, anesthetics, etc., and the bromine index is clearly required to be ≤100mgBr / 100g. Therefore, in order to rationally utilize reforming raffinate and give it a higher economic value, it is necessary to carry out hydrogenation deolefination and dearomatization treatment to remove the unsaturated hydrocarbons. At present, the representative hydrogenation deolefination and dearomatization catalysts are mainly divided into two categories: precious metals and non-precious metals. Ni, Pt, and Pd are the three most widely used metal catalysts. Pd hydrogenation performance K Pd The active K of Pt is 1 / 7 of that of metal Ni. Pt The price of palladium and platinum is several hundred times higher than that of nickel, and the requirements for sulfur, arsenic and other toxic substances in the raw materials are relatively high.

[0004] At present, the process flow of reforming raffinate oil to produce high value-added products varies according to the nature of the raw materials and product requirements, mainly including hydrogenation first and then fractionation, and fractionation first and then hydrogenation. When the benzene and olefin content is high, the process flow of hydrogenation first and then fractionation is basically adopted to ensure that the benzene content of the product meets the standard requirements; when the benzene and olefin content is low, the process flow of fractionation first and then hydrogenation is basically adopted. The hydrogenation operation load is small, but the hydrogen purity requirement is high. Due to the azeotropic phenomenon of components in the distillation process, the requirements for the number of plates and towers are different. At the same time, the nickel-based hydrogenation deolefination and debenzenization catalyst has poor thermal stability at high temperatures, NiO particles are easy to agglomerate and sinter, and there are problems such as poor dispersion and utilization rate. In addition, impurities such as sulfur, nitrogen and heavy metals in the raw materials are easy to cause catalyst poisoning, which affects the service life of the catalyst and increases the operating cost, so the raw materials need to be pretreated. Therefore, the existing process flow often has problems such as low utilization rate of reforming raffinate oil, single processed products, low product yield, short operating cycle of hydrogenation catalyst, and insensitivity to temperature increase. It is necessary to comprehensively consider multiple factors such as raw material properties, product types, catalyst stability and sulfur resistance, and distillation accuracy to achieve efficient utilization of reforming raffinate oil.

[0005] For the process of first fractionating and then hydrogenating, C5 and below components are prone to unqualified benzene and bromine index and cannot meet the requirements of pentane foaming agent if they are not treated with hydrogenation saturation, which is not suitable for raw materials with high benzene content; the C6 mixture in logistics II has the problem of low isomerization conversion rate; the hydrogenation and isomerization products are not separated by gas and liquid, resulting in a high light hydrocarbon component in isohexane during the subsequent fractionation process; the raw materials entering the hydrogenation reactor have not been treated with desulfurization, which is easy to cause poisoning and deactivation of the hydrogenation catalyst.

[0006] For the process of hydrogenation followed by separation, during distillation, sulfolane, water and impurities are discharged from the bottom of the tower, which can easily cause the loss of some heavy fractions and affect the yield of 120# solvent oil. At the same time, the C6 product at the top of the distillation tower is not distilled and separated, which can easily lead to a low yield of n-hexane and an inability to produce high-purity n-hexane with a price better than 6# solvent oil, and fail to achieve efficient utilization of the raffinate oil.

[0007] At the same time, there are documents or publicity reports that the process of producing solvent oil from reforming raffinate oil adopts a two-stage hydrogenation process for hydrodebenzening. The first stage uses a hydrodesulfurization catalyst to remove cyclopentane to protect the subsequent catalyst, and the second stage uses a high-nickel hydrogenation catalyst to remove benzene. However, since the hydrodesulfurization catalyst needs to be pre-sulfurized first and the second-stage catalyst needs to be pre-reduced first, the two cannot be operated at the same time, the startup process is cumbersome, and the residual sulfide oil in the first stage is bound to affect the second-stage catalyst. Therefore, a large amount of raw oil is required for flushing, affecting the start-up cycle of the device. Summary of the invention

[0008] In order to solve the above problems, the purpose of the present invention is to provide a hydrogenation catalyst and a preparation method thereof, and a method and system for producing solvent oil from reforming raffinate oil. The method is suitable for separating and utilizing reforming raffinate oil with high benzene and olefin content, and can utilize reforming raffinate oil to produce a variety of solvent oils, effectively increasing the added value of reforming raffinate oil.

[0009] In order to achieve the above-mentioned purpose, the present invention provides a hydrogenation catalyst, which includes a carrier and a first active metal component and a second active metal component loaded on the carrier, wherein the metal element of the first active metal component includes nickel, and the weight content of the first active metal component in the catalyst is 40-70%, based on the total weight of the catalyst as 100%, the weight content of the carrier (calculated as oxide) in the catalyst is 20-59%, and the balance is the second active metal component.

[0010] In a specific embodiment of the present invention, compared with existing nickel-based catalysts and hydrogenation catalysts, the hydrogenation catalyst provided by the present invention has a higher nickel content, and a higher dispersion of Ni metal, which can reach more than 10%, and has more hydrogenation active centers. Therefore, the hydrogenation catalyst has a better removal effect on benzene and olefins and the removal is more thorough.

[0011] In the above hydrogenation catalyst, the weight of the first active metal component in the catalyst is generally controlled to be 40-70%, for example, 40%, 45%, 50%, 55%, 60%, 65%, 70% or any two thereof.

[0012] In the above hydrogenation catalyst, the weight content of the carrier in the catalyst is 20-59%, for example, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 59% or a range consisting of any two thereof.

[0013] In a specific embodiment of the present invention, the specific surface area of ​​the hydrogenation catalyst is generally 200-500m 2 / g, for example 200m 2 / g, 250m 2 / g、300m 2 / g, 350m 2 / g, 400m 2 / g, 450m 2 / g、500m 2 / g or a range consisting of any two thereof.

[0014] In a specific embodiment of the present invention, the pore volume of the hydrogenation catalyst is generally 0.3-0.6 cm 3 / g, for example 0.3cm 3 / g, 0.35cm3 / g, 0.4cm 3 / g, 0.45cm 3 / g, 0.5cm 3 / g, 0.55cm 3 / g, 0.6cm 3 / g or a range consisting of any two thereof.

[0015] In a specific embodiment of the present invention, the carrier is generally an oxide, for example, it may include one of aluminum oxide, silicon oxide, titanium oxide, and cerium oxide, or it may include a mixture of at least one of silicon oxide, titanium oxide, and cerium oxide and aluminum oxide. That is, the carrier may include one or a combination of two or more of aluminum oxide, silicon oxide, titanium oxide, and cerium oxide, and the content of aluminum oxide is not zero.

[0016] In a specific embodiment of the present invention, the first active metal component and the second active metal component in the above catalyst are usually present in the form of metal oxides.

[0017] In a specific embodiment of the present invention, the metal element of the second active metal component may include one or a combination of two or more of copper, lanthanum, magnesium, etc. In a specific embodiment of the present invention, the nickel content, nickel dispersion and hydrogenation active center content in the catalyst can be increased by controlling the coprecipitation process and precipitation pH value of the metal active component during the catalyst preparation process.

[0018] The present invention further provides a method for preparing the above hydrogenation catalyst, the preparation method comprising:

[0019] The temperature of the carrier precursor slurry reaches the precipitation reaction temperature, and the pH value of the carrier precursor slurry is adjusted to an alkaline pH value (the pH value can be adjusted by adding a precipitant) to obtain a first mixed system;

[0020] Adding a first active metal component precursor, a second active metal component precursor, and a precipitant to the first mixed system simultaneously, maintaining the pH of the system at an alkaline pH value, to obtain a second mixed system;

[0021] The second mixed system is subjected to aging treatment, and the aging product is calcined to obtain the hydrogenation catalyst.

[0022] In the above preparation method, the carrier precursor is converted into a carrier of a hydrogenation catalyst after being dried and calcined. In a specific embodiment, the carrier precursor may include pseudo-boehmite, and the pseudo-boehmite is converted into alumina after being dried and calcined.

[0023] In the above preparation method, the nickel content, nickel dispersion and hydrogenation active center content in the catalyst can be increased by adjusting the type of the precursor of the first active metal component, the type of the precursor of the second active metal component and the type of the precipitant precursor.

[0024] In the above preparation method, the precipitant can not only be used to adjust the pH value, but also precipitate the metal elements in the first active metal component precursor and the metal elements in the second active metal component precursor. Specifically, the precipitant can include an alkaline precipitant, preferably a soluble carbonate, such as potassium carbonate and / or sodium carbonate.

[0025] In the above preparation method, the amount of the precipitant can be determined based on the pH value adjustment and the amount required to precipitate the metal element in the first active metal component precursor and the metal element in the second active metal component precursor.

[0026] In the above preparation method, the precursor of the first active metal component can be a compound of the metal element in the first active metal component, for example, a metal salt of the metal element in the first active metal component, preferably a soluble metal salt of the metal element in the first active metal component, for example, a nitrate of the metal element in the first active metal component, such as nickel nitrate.

[0027] In the above preparation method, the second active metal component precursor can be a compound of the metal element in the second active metal component, for example, a metal salt of the metal element in the second active metal component, preferably a soluble metal salt of the metal element in the second active metal component, for example, a nitrate of the metal element in the second active metal component, such as magnesium nitrate.

[0028] In the above preparation method, the amounts of the carrier precursor, the first active metal component precursor and the second active metal component precursor correspond to the weight contents of the carrier, the first active metal component and the second active metal component in the above hydrogenation catalyst.

[0029] In a specific embodiment of the invention, the first active metal component precursor and the second active metal component precursor can be added to the first mixed system in the form of a mixed solution of the two; the precipitant is also generally added to the first mixed reaction system in the form of a solution. By adding the mixed solution of the first active metal component precursor and the second active metal component precursor and the precipitant solution in parallel, and controlling the drop rate of the two mixed solutions, the nickel content, nickel dispersion and hydrogenation active center content in the catalyst can be effectively controlled. In a specific embodiment, the drop rate of the mixed solution of the first active metal component precursor and the second active metal component precursor is generally controlled to be 20-100ml / min, and the drop rate of the precipitant solution is generally controlled to be 10-300ml / min.

[0030] In the above preparation method, the alkaline pH value is 8-11, for example, 8, 9, 10, 11 or a range consisting of any two thereof.

[0031] In the above preparation method, the precipitation reaction temperature is 40-90°C, for example, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C or any two thereof.

[0032] In the above preparation method, the temperature of the aging treatment can be the same as or different from the precipitation reaction temperature. The temperature of the aging treatment is generally 40-90°C, such as 40°C, 50°C, 60°C, 70°C, 80°C, 90°C or any two thereof.

[0033] In the above preparation method, the aging treatment time is generally controlled to be 1-5 hours, such as 1 hour, 2 hours, 3 hours, 4 hours, 5 hours or the range of any two thereof.

[0034] In the above preparation method, the calcination temperature can generally be controlled to be 300-600°C, for example, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C or a range consisting of any two thereof.

[0035] In the above preparation method, the calcination time is generally 1-5 h, such as 1 h, 2 h, 3 h, 4 h, 5 h or a range consisting of any two thereof.

[0036] In a specific embodiment of the present invention, the preparation method generally further comprises filtering, washing and drying in sequence after the aging treatment and before the calcination.

[0037] In the above preparation method, the washing is generally stopped when the filtrate reaches neutrality. The filter cake is subsequently dried and calcined.

[0038] In the above preparation method, the drying temperature may be 100-130°C, for example, 100°C, 110°C, 120°C, 130°C or a range consisting of any two thereof.

[0039] In the above preparation method, the drying time is generally 1-5 hours, for example, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours or a range consisting of any two thereof.

[0040] According to a specific embodiment of the present invention, the preparation method of the above-mentioned hydrogenation catalyst may include:

[0041] The slurry formed by the carrier precursor and water is heated to the precipitation reaction temperature of 40-90°C while stirring, and an aqueous solution of a precipitant is added to the slurry to adjust the pH value of the system to 8-11, thereby obtaining a first mixed system; while maintaining stirring, a mixed aqueous solution of a first active metal component precursor and a second active metal component precursor (the mixed aqueous solution can be formed by mixing an aqueous solution of the first active metal component precursor and an aqueous solution of the second active metal component precursor) and an aqueous solution of a precipitant are added to the first mixed system at the same time, and the pH value of the system is maintained at 8-11, thereby obtaining a second mixed system; the second mixed system is subjected to an aging treatment at 40-90°C for 1-5h, filtered and washed until the filtrate is neutral, and the filter cake is dried and calcined at 300-600°C for 1-5h to obtain the hydrogenation catalyst.

[0042] The present invention also provides a method for producing solvent oil by reforming raffinate oil, the method comprising:

[0043] S2, using a hydrogenation catalyst to catalyze the desulfurized and dehydrated reforming raffinate oil to perform hydrogenation debenzenization and deolefination reactions to obtain a reaction product; wherein the hydrogenation catalyst includes the above-mentioned hydrogenation catalyst;

[0044] S3, performing gas-liquid separation on the reaction product obtained in S2;

[0045] S4, distilling the separated liquid to respectively distill out C5 component, C6 component and components above C7;

[0046] S5, distilling the C6 component to respectively distill out cyclohexane and a mixture of normal hexane and isohexane;

[0047] S6. Distilling the mixture of normal hexane and isohexane to separate isohexane and normal hexane, thereby completing the production of solvent oil.

[0048] In a specific embodiment of the present invention, in the reforming raffinate oil that has not been desulfurized or dehydrated, the sulfur content is less than 20 mg / kg, the benzene content is 3-5v%, the olefin content is 1-3v%, and the total content of n-hexane and isohexane is greater than 50v%.

[0049] In a specific embodiment of the present invention, the above method further comprises: S1, desulfurizing and dehydrating the reforming raffinate oil, and the product S is ≤1 mg / kg.

[0050] In a specific embodiment of the present invention, in S1, the space velocity during the desulfurization and dehydration process is 1-10h -1 ;

[0051] In a specific embodiment of the present invention, the adsorbent used in the desulfurization and dehydration process in S1 includes a molecular sieve adsorbent, such as one or a combination of two or more of 3A molecular sieve, 4A molecular sieve, 5A molecular sieve and 13A molecular sieve;

[0052] In a specific embodiment of the present invention, the specific surface area of ​​the molecular sieve adsorbent used in S1 is generally 400-700m 2 / g. The pore volume of molecular sieve adsorbent is generally 0.05-0.30cm 3 / g.

[0053] In a specific embodiment of the present invention, in S2, the hydrogenation catalyst can effectively remove benzene and olefins in the reforming raffinate. According to a specific embodiment of the present invention, in the reaction product obtained in S2, the benzene content is ≤0.01%, and the bromine index is ≤50mgBr / 100g.

[0054] In a specific embodiment of the present invention, in S2, the conditions of the hydrodebenzenization and deolefination reactions can generally be controlled as follows: temperature 90-200°C, reaction pressure 1.0-3.0 MPa, hydrogen-oil volume ratio 100-300:1, volume space velocity 1.0-3.0 h -1 ;

[0055] In a specific embodiment of the present invention, in S4, the distillation pressure is generally 0-0.2 MPa.

[0056] In a specific embodiment of the present invention, the distillation process of S4 can be completed in a distillation tower, and the top temperature of the distillation tower can be 30-50°C, the bottom temperature can be 90-110°C, and the pressure in the tower can be 0-0.2MPa.

[0057] In a specific embodiment of the present invention, in S5, the distillation pressure is generally 0-0.1 MPa.

[0058] In a specific embodiment of the present invention, the distillation process of S5 can be completed in a distillation tower, the top temperature of the distillation tower is 55-75°C, the bottom temperature of the tower is 70-90°C, and the pressure in the tower is 0-0.1 MPa.

[0059] In a specific embodiment of the present invention, in S6, the distillation pressure is 0-0.1 MPa.

[0060] In a specific embodiment of the present invention, the distillation process of S6 can be completed in a distillation tower, the top temperature of the distillation tower is 50-70°C, the bottom temperature is 60-80°C, and the pressure in the tower is 0-0.1 MPa.

[0061] In a specific embodiment of the present invention, the isohexane obtained in S6 can be directly output as 6# solvent oil. According to actual needs, the isohexane obtained in S6 can also be converted into normal-hexane through a normalization reaction, and the purity of the normal-hexane product is ≥80%.

[0062] In a specific embodiment of the present invention, the method further comprises: S7, converting the isohexane obtained in S6 into normal-hexane through a normalization reaction.

[0063] In a specific embodiment of the present invention, in S7, the conditions of the normalization reaction are: reaction temperature 200-400°C, reaction pressure 1.0-3.0 MPa, hydrogen-oil volume ratio 100-300:1, volume space velocity 1.0-3.0 h -1 .

[0064] In a specific embodiment of the present invention, in S7, the catalyst for the normalization reaction may be a molecular sieve catalyst. Specifically, the molecular sieve catalyst may include a third active metal component, a non-molecular sieve carrier and a molecular sieve carrier.

[0065] In the above molecular sieve catalyst, the molecular sieve carrier includes one or a combination of two or more of MOR, MCM-41, ZSM-22, and SAPO-11.

[0066] In the above molecular sieve catalyst, the metal element of the third active metal component may include elements in Group VIB and / or Group VIII. In a specific embodiment, the third active metal component is usually present in the form of a metal oxide.

[0067] In the above molecular sieve catalyst, the non-molecular sieve carrier comprises alumina.

[0068] In the above molecular sieve catalyst, taking the total weight of the molecular sieve catalyst as 100%, the weight of the molecular sieve carrier accounts for 10-80% of the total weight of the catalyst, the weight of the third active metal component (in terms of oxide) accounts for 0.01-5% (e.g. 0.1-0.5%) of the total weight of the catalyst, and the remainder is non-molecular sieve carrier.

[0069] In a specific embodiment of the present invention, in S7, the purity of the raw material isohexane for the normalization reaction is above 90%, preferably above 95%.

[0070] In a specific embodiment of the present invention, the method for producing solvent oil by reforming raffinate oil may specifically include:

[0071] S1. Desulfurizing and dehydrating the reforming raffinate oil by using a molecular sieve adsorbent;

[0072] S2, using a hydrogenation catalyst to catalyze the desulfurized and dehydrated reforming raffinate oil to perform hydrogenation debenzenization and deolefination reactions to obtain a reaction product; wherein the hydrogenation catalyst includes the above-mentioned hydrogenation catalyst;

[0073] S3, performing gas-liquid separation on the reaction product obtained in S2, and outputting hydrogen-rich gas and liquid;

[0074] S4, distilling the separated liquid to separate C5 component (which can be used as pentane foaming agent), C6 component and components above C7 (which can be used as 120# solvent oil);

[0075] S5, distilling the C6 component to respectively distill out cyclohexane and a mixture of normal hexane and isohexane;

[0076] S6, distilling the mixture of normal hexane and isohexane to respectively distill out isohexane and normal hexane;

[0077] S7, converting the isohexane obtained in S6 into normal-hexane through a normalization reaction to complete the production of solvent oil.

[0078] The present invention also provides a system for producing solvent oil by reforming raffinate oil, and the system can realize the method for producing solvent oil by reforming raffinate oil.

[0079] In a specific embodiment of the present invention, the system for producing solvent oil by reforming raffinate oil comprises a desorption desulfurization reactor, a hydrogenation reactor, a first gas-liquid separator, a first distillation tower, a second distillation tower, and a third distillation tower connected in sequence.

[0080] The connection relationship of each device in the above system can be: the inlet of the desorption desulfurization reactor is used to receive the reforming raffinate oil, and the inlet is generally located at the top of the tower;

[0081] The outlet of the desorption desulfurization reactor at the bottom of the tower is connected to the inlet of the hydrogenation reactor (located at the top of the tower);

[0082] The outlet of the hydrogenation reactor at the bottom of the tower is connected to the inlet (located on the side line) of the first gas-liquid separator;

[0083] The outlet of the first gas-liquid separator at the bottom of the tower is connected to the inlet (located at the side line) of the first distillation tower;

[0084] The outlet of the first distillation tower located at the measuring line is connected to the inlet of the second distillation tower;

[0085] The outlet of the second distillation tower at the top of the tower is connected to the inlet of the third distillation tower;

[0086] The outlet of the third distillation tower at the top is used to output isohexane.

[0087] In the above system, the outlet of the first gas-liquid separator at the top of the tower is used to output hydrogen, the outlet of the first distillation tower at the top of the tower is used to output C5 components, the outlet of the first distillation tower at the bottom of the tower is used to output components above C7, the outlet of the first distillation tower at the measuring line is used to output C6 components, the outlet of the second distillation tower at the top of the tower is used to output a mixture of normal hexane and isohexane, the outlet of the second distillation tower at the bottom of the tower is used to output cyclohexane, the outlet of the third distillation tower at the bottom of the tower is used to output normal hexane, and the outlet of the third distillation tower at the top of the tower is used to output isohexane.

[0088] In a specific embodiment of the present invention, the system for producing solvent oil by reforming raffinate oil also includes a normalization reactor and a second gas-liquid separator, the inlet of the normalization reactor is connected to the outlet of the third distillation tower located at the top of the tower, the outlet of the normalization reactor is connected to the inlet of the second gas-liquid separator (located on the side line), the outlet of the second gas-liquid separator located at the top of the tower is used to output hydrogen, and the outlet of the second gas-liquid separator located at the bottom of the tower is used to output n-hexane.

[0089] In a specific embodiment of the present invention, the system may further include a hydrogen pipeline for supplying hydrogen to the hydrogenation reactor and / or the normalization reactor. The hydrogen pipeline may be provided with a circulating hydrogen compressor, the inlet of which may be connected to the gas outlet of the first gas-liquid separator and / or the second gas-liquid separator, that is, the compressor may be supplied with gas by the first gas-liquid separator and the second gas-liquid separator.

[0090] The beneficial effects of the present invention are:

[0091] 1. The method provided by the present invention pre-treats the raw materials by loading a molecular sieve adsorbent in an adsorption reactor to perform desulfurization, dehydration and impurity removal to solve the problem of poisoning of the subsequent hydrodebenzening catalyst caused by sulfolane in the reforming raffinate raw material in the prior art, effectively protects the service life of the subsequent hydrodeolefination and debenzening unit high-nickel hydrogenation catalyst, extends the operation cycle of the device, reduces the increase in operating costs due to frequent replacement of catalysts, and the separated C7 and above components meet the sulfur content requirements of 120# solvent oil; at the same time, it avoids the problem in the prior art that the hydrodesulfurization catalyst needs to be pre-sulfurized, resulting in a cumbersome device startup process, and the residual sulfide oil is difficult to replace, affecting the device startup cycle.

[0092] 2. The method provided by the present invention can set up distillation units step by step from the perspective of molecular refining according to the composition and boiling point of raw materials, and utilize the normalization reaction of isohexane to improve the purity and yield of normal hexane, produce normal hexane, pentane foaming agent and 120# solvent oil, and realize the efficient utilization of reforming raffinate oil. It effectively solves the problems of low utilization rate of reforming raffinate oil, single processed products, and low product yield.

[0093] 3. The nickel-based hydrogenation catalyst provided by the present invention can achieve high dispersion of high-content nickel active components on the carrier alumina, carry out hydrogenation deolefination and debenzenization reactions on the reforming raffinate oil, and ensure the operation cycle of the hydrogenation device. BRIEF DESCRIPTION OF THE DRAWINGS

[0094] Figure 1 The present invention provides a process flow chart and a schematic diagram of system connection for producing solvent oil from reformed raffinate oil.

[0095] Explanation of symbols

[0096] Adsorption desulfurization reactor 1, hydrogenation reactor 2, first gas-liquid separator 3, first distillation tower 4, second distillation tower 5, third distillation tower 6, normalization reactor 7, second gas-liquid separator 8, circulating hydrogen compressor 9. DETAILED DESCRIPTION

[0097] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.

[0098] In the following examples and comparative examples, the metal dispersion of the hydrogenation catalyst was measured in a static chemical adsorption instrument with H2 as the adsorption gas. The specific measurement method is as follows:

[0099] The sample was degassed at 130°C, then H2 reduced at 400°C, cooled to 35°C for the first saturated adsorption, and then vacuumed for the second saturated adsorption. The difference between the two saturated adsorptions is the volume of chemically adsorbed hydrogen.

[0100] Metal dispersion calculation formula:

[0101]

[0102] In the formula, V H2 is the volume of chemically adsorbed hydrogen, in L, W is the total mass of the catalyst, in g, P is the percentage of Ni, M Ni is the molecular mass of Ni.

[0103] Example 1a

[0104] This embodiment provides a hydrogenation catalyst, and the preparation method thereof comprises:

[0105] Step 1, 11.50 g of pseudo-boehmite powder (containing 70 wt% of Al2O3) and 40 ml of deionized water were mixed and stirred to obtain a first slurry;

[0106] Dissolve 58.16g of nickel nitrate hexahydrate in deionized water and adjust the volume to 200ml to prepare a 1mol / L nickel nitrate solution; dissolve 12.82g of magnesium nitrate hexahydrate in deionized water and adjust the volume to 50ml to prepare a 1mol / L magnesium nitrate solution. Measure 184.7ml of the 1mol / L nickel nitrate solution and 28.5ml of the 1mol / L magnesium nitrate solution and mix them evenly to obtain a second solution;

[0107] Dissolve 207.32 g of anhydrous potassium carbonate in deionized water and adjust the volume to 1000 ml to prepare a 1.5 mol / L potassium carbonate solution. Measure 665.3 ml of the 1.5 mol / L potassium carbonate solution as the third solution.

[0108] Step 2, adding the first slurry into the reactor, starting the stirring speed at 200 rpm, heating to the reaction temperature of 60° C., adding 1.3 ml of the third solution into the reactor, adjusting the pH of the first slurry to 10, and forming a first mixed system;

[0109] Under stirring conditions, the second solution and the third solution were added to the first mixed system at 35 ml / min and 109.2 ml / min respectively, and the pH value was controlled to be constant at 10. After the second solution and the third solution were added dropwise, a second mixed system was obtained.

[0110] Step 3, stirring and aging the second mixed system at 60° C. for 2 h. After aging, filtering to obtain a filter cake and washing to neutrality, drying the filter cake in an oven at 120° C. for 4 h, grinding and calcining in a muffle furnace at 500° C. for 5 h to obtain a nickel hydrogenation catalyst.

[0111] In the above hydrogenation catalyst, the mass content of nickel oxide is 60%, and the mass content of magnesium oxide is 5%.

[0112] The catalyst of this example was tested and the Ni metal dispersion was found to be 15.08% and the specific surface area was 251 m 2 / g, the pore volume of the hydrogenation catalyst is 0.41cm 3 / g.

[0113] Example 1b

[0114] This embodiment provides a hydrogenation catalyst, and the preparation method thereof comprises:

[0115] Step 1, 16.10 g of pseudo-boehmite powder (containing 70 wt% of Al2O3), 2.30 g of silicon oxide and 55 ml of deionized water were mixed and stirred to obtain a first slurry;

[0116] Dissolve 72.70g of nickel nitrate hexahydrate in deionized water and adjust the volume to 500ml to prepare a 0.5mol / L nickel nitrate solution; dissolve 4.33g of lanthanum nitrate hexahydrate in deionized water and adjust the volume to 20ml to prepare a 0.5mol / L lanthanum nitrate solution. Measure 246.3ml of the 0.5mol / L nickel nitrate solution and 2.8ml of the 0.5mol / L lanthanum nitrate solution and mix them evenly to obtain a second solution;

[0117] Dissolve 15.81 g of ammonium bicarbonate in deionized water and adjust the volume to 200 ml to prepare a 1 mol / L ammonium bicarbonate solution. Measure 191.1 ml of the 1 mol / L ammonium bicarbonate solution as the third solution.

[0118] Step 2, adding the first slurry into the reactor, starting the stirring speed at 200 rpm, heating to the reaction temperature of 80° C., adding 1.2 ml of the third solution into the reactor, adjusting the pH of the first slurry to 8, and forming a first mixed system;

[0119] Under stirring conditions, the second solution and the third solution were added to the first mixed system at 20 ml / min and 15 ml / min respectively, and the pH value was controlled to be constant at 8. After the second solution and the third solution were added dropwise, a second mixed system was obtained.

[0120] Step 3: Stir and age the second mixed system at 80° C. for 3 h. After aging, filter to obtain a filter cake, wash it to neutrality, dry it in an oven at 120° C. for 4 h, grind it, and calcine it in a muffle furnace at 500° C. for 5 h to obtain a nickel hydrogenation catalyst.

[0121] In the above hydrogenation catalyst, the mass content of nickel oxide is 70%, and the mass content of lanthanum oxide is 1%.

[0122] The catalyst of this example was tested and the Ni metal dispersion was found to be 16.18% and the specific surface area was 246 m 2 / g, the pore volume of the hydrogenation catalyst is 0.40cm 3 / g.

[0123] Example 1c

[0124] This embodiment provides a hydrogenation catalyst, and the preparation method thereof comprises:

[0125] Step 1, 11.50 g of pseudo-boehmite powder (containing 70 wt% of Al2O3) and 40 ml of deionized water were mixed and stirred to obtain a first slurry;

[0126] 58.16 g of nickel nitrate hexahydrate was dissolved in deionized water and the volume was adjusted to 200 ml to prepare a 1 mol / L nickel nitrate solution; 4.83 g of copper nitrate trihydrate was dissolved in deionized water and the volume was adjusted to 20 ml to prepare a 1 mol / L copper nitrate solution; 184.7 ml of the 1 mol / L nickel nitrate solution and 14.5 ml of the 1 mol / L copper nitrate solution were measured and mixed to obtain a second solution;

[0127] Dissolve 207.32 g of anhydrous potassium carbonate in deionized water and adjust the volume to 1000 ml to prepare a 1.5 mol / L potassium carbonate solution. Measure 621.4 ml of the 1.5 mol / L potassium carbonate solution as the third solution.

[0128] Step 2, adding the first slurry into the reactor, starting the stirring speed at 100 rpm, heating to a reaction temperature of 60° C., adding 1.3 ml of the third solution into the reactor, adjusting the pH of the first slurry to 10, and forming a first mixed system;

[0129] Under stirring conditions, the second solution and the third solution were added to the first mixed system at 35 ml / min and 109 ml / min respectively, and the pH value was controlled to be constant at 10. After the second solution and the third solution were added dropwise, a second mixed system was obtained.

[0130] Step 3, stirring and aging the second mixed system at 60°C for 2 hours. After aging, filter to obtain a filter cake and wash it to neutrality. Place the filter cake in a 120°C oven and dry it for 4 hours. After grinding, calcine it in a muffle furnace at 500°C for 5 hours, and reduce it at 400°C for 10 hours under high-purity H2 to obtain a nickel hydrogenation catalyst.

[0131] In the above hydrogenation catalyst, the mass content of nickel oxide is 60%, and the mass content of copper oxide is 5%.

[0132] The catalyst of this example was tested and the Ni metal dispersion was found to be 14.74% and the specific surface area was 248 m 2 / g, the pore volume of the hydrogenation catalyst is 0.42cm 3 / g.

[0133] The method for producing solvent oil by reforming raffinate oil in Examples 2a to 2e is as follows: Figure 1 The system shown in the figure includes a desorption desulfurization reactor 1, a hydrogenation reactor 2, a first gas-liquid separator 3, a first distillation tower 4, a second distillation tower 5, a third distillation tower 6, a normalization reactor 7, a second gas-liquid separator 8, and a circulating hydrogen compressor 9.

[0134] Among them, the desorption desulfurization reactor 1 has an inlet at the top and an outlet at the bottom; the hydrogenation reactor 2 has an inlet at the top and an outlet at the bottom; the first gas-liquid separator 3 has an inlet at the line, and outlets are provided at the bottom and the top respectively; the first distillation tower 4 has an inlet at the line, and outlets are provided at the top and the bottom respectively; the second distillation tower 5 has an inlet at the line, and outlets are provided at the top and the bottom respectively; the third distillation tower 6 has an inlet at the line, and outlets are provided at the top and the bottom respectively; the normalization reactor 7 has an inlet at the top and an outlet at the bottom; the second gas-liquid separator 8 has an inlet at the line, and outlets are provided at the top and the bottom respectively. The circulating hydrogen compressor 9 has an inlet and an outlet.

[0135] Specifically, the connection relationship between the various devices is as follows: the outlet of the desorption desulfurization reactor 1 at the bottom of the tower is connected to the inlet of the hydrogenation reactor 2 (located at the top of the tower); the outlet of the hydrogenation reactor 2 at the bottom of the tower is connected to the inlet of the first gas-liquid separator 3; the outlet of the first gas-liquid separator 3 at the bottom of the tower is connected to the inlet of the first distillation tower 4; the outlet of the first distillation tower 4 at the measuring line is connected to the inlet of the second distillation tower 5; the outlet of the second distillation tower 5 at the top of the tower is connected to the inlet of the third distillation tower 6; the outlet of the third distillation tower 6 at the top of the tower is connected to the inlet of the normalization reactor 7; the outlet of the normalization reactor 7 at the bottom of the tower is connected to the inlet of the second gas-liquid separator 8, and the outlet of the second gas-liquid separator 8 at the top of the tower and the outlet of the first gas-liquid separator 3 at the top of the tower are respectively connected to the inlet of the circulating hydrogen compressor 9; the outlet of the circulating hydrogen compressor 9 is respectively connected to the inlet of the hydrogenation reactor 2 and the inlet of the normalization reactor 7.

[0136] The process flow of the method for producing solvent oil from reformed raffinate oil used in Examples 2a to 2e is as follows: Figure 1 As shown, specifically including:

[0137] S1, transporting the reforming raffinate oil to an adsorption reactor for desulfurization and dehydration;

[0138] S2, the desulfurization and dehydration products are mixed with hydrogen and enter the hydrogenation reactor to remove benzene and olefins, wherein the hydrogenation catalyst loaded in the hydrogenation reactor is the hydrogenation catalyst provided by the present invention;

[0139] S3, transporting the hydrogenation reaction product to a gas-liquid separator for gas-liquid separation, the separated liquid product is discharged from the bottom of the gas-liquid separator, and the separated hydrogen-rich gas is discharged from the top of the gas-liquid separator. The hydrogen-rich gas can be mixed with new hydrogen and used as circulating hydrogen after being pressurized by a circulating hydrogen compressor;

[0140] S4, the liquid product separated from the gas and liquid enters the first distillation tower, the top of the tower is C5 component (pentane foaming agent), the side line is C6 component, and the bottom of the tower is C7 and above components (120# solvent oil);

[0141] S5, the C6 component from the side line of the first distillation tower enters the second distillation tower for fractionation, the top of the tower is a mixture of normal hexane and isohexane, and the bottom of the tower is cyclohexane;

[0142] S6, the mixture of normal hexane and isohexane enters the third distillation tower for fractionation, with isohexane at the top and normal hexane at the bottom;

[0143] S7. Isohexane enters the normalization reactor for reaction, and the obtained product enters the separator for gas-liquid separation. The bottom product of the separator is high-concentration n-hexane, which is then mixed with the n-hexane product at the bottom of the third distillation tower to further improve the n-hexane yield.

[0144] Table 1 shows the composition of the reforming raffinate oil feedstock in the following Examples 2a to 2e, Comparative Example 1, and Comparative Example 2.

[0145] Table 1

[0146]

[0147]

[0148] Example 2a

[0149] This embodiment provides a method for producing solvent oil by reforming raffinate oil, comprising:

[0150] S1. Using the reforming raffinate oil in Table 1 as raw material, the reforming raffinate oil enters the adsorption reactor for desulfurization and dehydration, and the catalyst used is industrial 5A molecular sieve adsorbent;

[0151] S2, the desulfurization and dehydration products are mixed with hydrogen and enter the hydrogenation reactor to remove benzene and olefins, and the catalyst used is the high nickel hydrogenation catalyst (Ni metal dispersion is greater than 10%) prepared in Example 1a;

[0152] Adsorption desulfurization reaction conditions: normal temperature, normal pressure, space velocity of 3h -1 , product S≤1mg / kg;

[0153] S3, the product of the hydrogenation reactor enters the separator for gas-liquid separation, the liquid product is discharged from the bottom of the tower, and the hydrogen-rich gas is discharged from the top. The hydrogen-rich gas can be mixed with the new hydrogen of the reforming unit and used as circulating hydrogen after being pressurized by the circulating hydrogen compressor;

[0154] Fixed bed hydrogenation reactor reaction conditions: reaction temperature 120 ° C, reaction pressure 1.0 MPa, hydrogen oil volume ratio 100: 1, volume space velocity 3.0 h -1 , the benzene removal rate was measured to be 100%;

[0155] S4, the liquid product at the bottom of the separator enters the first distillation tower, the top of the tower is C5 component, the line discharges C6 component, and the bottom of the tower is C7 and above components;

[0156] The operating conditions of the first distillation tower are as follows: the pressure in the tower is 0.1 MPa, the temperature at the top of the tower is 35°C, the temperature at the bottom of the tower is 95°C, the C5 component at the top of the tower is pentane foaming agent, the C7 and above components at the bottom of the tower are 120# solvent oil, and the C6 component is discharged from the side line; the bromine index is determined by using a bromine index tester based on the principle of microcoulomb titration. The bromine index of the C5 component is 5.1 mgBr / 100g, and the bromine index of the C7 and above components is 9.8 mgBr / 100g;

[0157] S5, the C6 component coming out of the side line enters the second distillation tower for fractionation, the top of the tower is a mixture of n-hexane and isohexane, and the bottom of the tower is cyclohexane;

[0158] The operating conditions of the second distillation tower are as follows: the top pressure is 0.1 MPa, the top temperature is 60°C, the bottom temperature is 72°C, and the purity of cyclohexane at the bottom is 97 wt%;

[0159] S6, the mixture of normal hexane and isohexane enters the third distillation tower for fractionation, with isohexane at the top and normal hexane at the bottom;

[0160] The operating conditions of the third distillation tower are: top pressure 0.1MPa, top temperature 55°C, bottom temperature 65°C, and n-hexane purity at the bottom 87%;

[0161] S7. The top product isohexane enters the normalization reactor for reaction, and the obtained product enters the separator for gas-liquid separation. The bottom product of the separator is high-concentration n-hexane, which is then mixed with the n-hexane product at the bottom of the third distillation tower to further improve the n-hexane yield.

[0162] The reaction conditions of the normalization reactor are: reaction temperature 380°C, reaction pressure 2.0MPa, hydrogen-oil volume ratio 200:1, volume space velocity 1.5h -1 , conversion rate 91%, selectivity> 99wt%;

[0163] Among them, the catalyst used in the normalization reaction is a molecular sieve catalyst, which is composed of a molecular sieve carrier, a non-molecular sieve carrier and a third active metal component. Among them, the molecular sieve carrier is a mercerized molecular sieve MOR, and its weight content in the catalyst is 80%; the third active metal component is palladium oxide, and its weight content in the catalyst is 0.35%; the remainder is aluminum oxide as a non-molecular sieve catalyst.

[0164] The products obtained in this embodiment are as follows: the purity of n-hexane is 83wt%, and the yield is 54%; the purity of cyclohexane is>97wt%; the C5 component meets the standard requirements of pentane foaming agent; and the C7 and above components meet the standard requirements of 120# solvent oil.

[0165] The above benzene removal rate, conversion rate, selectivity, purity of each component in the product and yield are obtained by analyzing the raw material and product group composition by gas chromatography.

[0166] Example 2b

[0167] This embodiment provides a method for producing solvent oil by reforming raffinate oil, comprising:

[0168] The raw materials, process flow, adsorption desulfurization reaction, hydrogenation reaction and normalization reaction conditions are exactly the same as those in Example 2a, except that the operating conditions of the three distillation towers are changed.

[0169] The operating conditions of the first distillation tower are as follows: the pressure in the tower is 0.1 MPa, the temperature at the top of the tower is 40°C, the temperature at the bottom of the tower is 102°C, the C5 component at the top of the tower is pentane foaming agent, and the bromine index is 5.8 mgBr / 100g, and the C7 and above components at the bottom of the tower are 120# solvent oil, and the bromine index is 8.3 mgBr / 100g;

[0170] The operating conditions of the second distillation tower are as follows: the top pressure is 0.1 MPa, the top temperature is 66°C, the bottom temperature is 78°C, and the purity of cyclohexane at the bottom is 99 wt%;

[0171] The operating conditions of the third distillation tower are: top pressure 0.1MPa, top temperature 60°C, bottom temperature 71°C, and n-hexane purity at the bottom 91%;

[0172] The products obtained in this embodiment are as follows: the purity of n-hexane is 88wt%, and the yield is 53%; the purity of cyclohexane is>99wt%; the C5 component meets the standard requirements of pentane foaming agent; and the C7 and above components meet the standard requirements of 120# solvent oil.

[0173] Example 2c

[0174] This embodiment provides a method for producing solvent oil by reforming raffinate oil, comprising:

[0175] The raw materials, process flow, adsorption desulfurization reaction, hydrogenation reaction and normalization reaction conditions used are exactly the same as those in Example 2b, except that the operating conditions of the three distillation towers are changed.

[0176] The operating conditions of the first distillation tower are as follows: the pressure in the tower is 0.1 MPa, the temperature at the top of the tower is 50°C, the temperature at the bottom of the tower is 110°C, the C5 component at the top of the tower is pentane foaming agent, and the bromine index is 7.8 mgBr / 100g, and the C7 and above components at the bottom of the tower are 120# solvent oil, and the bromine index is 8.9 mgBr / 100g;

[0177] The operating conditions of the second distillation tower are as follows: the top pressure is 0.1 MPa, the top temperature is 75°C, the bottom temperature is 90°C, and the purity of cyclohexane at the bottom is 98 wt%;

[0178] The operating conditions of the third distillation tower are: top pressure 0.1MPa, top temperature 65°C, bottom temperature 78°C, and n-hexane purity at the bottom 88%;

[0179] The products obtained in this embodiment are as follows: the purity of n-hexane is 85wt%, and the yield is 51%; the purity of cyclohexane is>98wt%; the C5 component meets the standard requirements of pentane foaming agent; and the C7 and above components meet the standard requirements of 120# solvent oil.

[0180] Example 2d

[0181] This embodiment provides a method for producing solvent oil by reforming raffinate oil:

[0182] The raw materials, process flow, distillation tower operating conditions, adsorption desulfurization reaction and normalization reaction conditions are exactly the same as those in Example 2b, except for the fixed bed hydrogenation reaction conditions.

[0183] Fixed bed hydrogenation reactor reaction conditions: reaction temperature 180°C, reaction pressure 1.0MPa, hydrogen-oil volume ratio 100:1, volume space velocity 3.0h -1 , benzene removal rate 100%;

[0184] Products of the first distillation tower: The bromine index of the C5 component at the top of the tower is 1.2 mgBr / 100g, which meets the requirements of pentane foaming agent; the bromine index of the C7 and above components at the bottom of the tower is 3.5 mgBr / 100g, which meets the requirements of 120# solvent oil;

[0185] The obtained products: the purity of n-hexane is 88wt%, and the yield is 53%; the purity of cyclohexane is>99wt%; the C5 component meets the standard requirements of pentane foaming agent; and the C7 and above components meet the standard requirements of 120# solvent oil.

[0186] Example 2e

[0187] This embodiment provides a method for producing solvent oil by reforming raffinate oil:

[0188] The raw materials, process flow, distillation tower operating conditions, adsorption desulfurization reaction and fixed bed hydrogenation reaction conditions are exactly the same as those in Example 2b, except for the normalization reaction conditions.

[0189] The reaction conditions of the normalization reactor are: reaction temperature 300°C, reaction pressure 2.0 MPa, hydrogen-oil volume ratio 200:1, volume space velocity 1.5 h -1 , conversion rate 73%, selectivity> 99wt%;

[0190] The obtained products: the purity of n-hexane is 82wt%, and the yield is 52%; the purity of cyclohexane is>99wt%; the C5 component meets the standard requirements of pentane foaming agent; and the C7 and above components meet the standard requirements of 120# solvent oil.

[0191] Comparative Example 1

[0192] This comparative example provides a method for producing solvent oil by reforming raffinate oil:

[0193] The raw materials, process flow, distillation tower operating conditions, adsorption desulfurization reaction and normalization reaction conditions are exactly the same as those in Example 2b, except for the fixed bed hydrogenation reaction conditions.

[0194] Fixed bed hydrogenation reactor reaction conditions: reaction temperature 80 ° C, reaction pressure 1.0 MPa, hydrogen oil volume ratio 100: 1, volume space velocity 3.0 h -1 , benzene removal rate 83%;

[0195] The first distillation tower product: the bromine index of the C5 component at the top of the tower is 121.2 mgBr / 100g, which does not meet the requirements of the pentane foaming agent; the bromine index of the C7 and above components at the bottom of the tower is 133.7 mgBr / 100g, which does not meet the requirements of 120# solvent oil;

[0196] The products obtained in this comparative example are: n-hexane with a purity of 76wt% and a yield of 53%; and cyclohexane with a purity of >99w%.

[0197] Comparative Example 2

[0198] This comparative example provides a method for producing solvent oil by reforming raffinate oil, the raw materials used are the same as those in Example 2b, and the method comprises:

[0199] 1. The reforming raffinate raw material is firstly hydrogenated in a reactor to remove benzene and olefins, and the catalyst used is a conventional hydrogenation deolefination catalyst;

[0200] The reaction conditions of the hydrogenation reactor are: reaction temperature 120°C, reaction pressure 1.0MPa, hydrogen to oil volume ratio 100:

[0201] 1. Volumetric airspeed 3.0h -1 , benzene removal rate 82%;

[0202] The preparation method is as follows: weigh 82.9g of aluminum nitrate nonahydrate, adjust the volume to 240ml, and prepare a 1mol / L aluminum nitrate solution. Measure 190ml of 1mol / L nickel nitrate solution, 30ml of 1mol / L magnesium nitrate solution, and 170ml of 1mol / L aluminum nitrate solution and mix them evenly to form a metal mixed solution for standby use. Measure 1.5mol / L potassium carbonate as 1000ml of precipitant solution for standby use. Add 40ml of clean water to the reactor, turn on the stirring speed of 250rmp, and heat to the reaction temperature of 50°C. Under stirring conditions, add the metal mixed solution and the precipitant solution at 35ml / min and 71ml / min respectively, and control the pH value to be constant at 9. After the solution is added dropwise, stir and age at 50°C for 2h. Filter the obtained material and wash until the filtrate is neutral. Place the filter cake in an oven at 120°C and dry it for 4h. After grinding, roast it in a muffle furnace at 500°C for 5h and grind it to obtain the catalyst.

[0203] 2. The hydrogenation reaction product enters the separator for gas-liquid separation, the liquid product is discharged from the bottom, and the hydrogen-rich gas discharged from the top is mixed with the new hydrogen from the reforming unit and used as circulating hydrogen after being pressurized by the circulating hydrogen compressor;

[0204] 3. The liquid product at the bottom of the separator enters the first distillation tower for fractionation, the C5 component is discharged from the top of the tower, the C6 component is discharged from the side line, and the C7 and above components are discharged from the bottom of the tower;

[0205] The operating conditions of the first distillation tower are as follows: the pressure in the tower is 0.1 MPa, the temperature at the top of the tower is 40°C, the temperature at the bottom of the tower is 102°C, the C5 component at the top of the tower is a pentane foaming agent, and the bromine index is 131.1 mgBr / 100g, which does not meet the requirements of the pentane foaming agent; the bromine index of the C7 and above components at the bottom of the tower is 138.9 mgBr / 100g, which does not meet the requirements of 120# solvent oil;

[0206] 4. The C6 component enters the second distillation tower for fractionation, with a mixture of n-hexane and isohexane at the top and cyclohexane at the bottom;

[0207] The operating conditions of the second distillation tower are as follows: the top pressure is 0.1 MPa, the top temperature is 66°C, the bottom temperature is 78°C, and the purity of cyclohexane at the bottom is 98 wt%;

[0208] 5. The mixture of n-hexane and isohexane enters the third distillation tower for fractionation, with isohexane at the top and n-hexane at the bottom;

[0209] The operating conditions of the third distillation tower are: top pressure 0.1 MPa, top temperature 60°C, and bottom temperature 71°C.

[0210] The products obtained in this comparative example are: n-hexane with a purity of 88wt% and a yield of 31%; isohexane with a purity of 91wt% (which can be used as 6# solvent oil), and cyclohexane with a purity of>99wt%.

[0211] Table 2 shows the evaluation results of the products of Example 2a-Example 2e and Comparative Example 1-Comparative Example 2.

[0212] Table 2

[0213]

[0214] It can be seen from Table 2 that the evaluation results of Examples 2a to 2e are significantly better than those of Comparative Examples 1 and 2. The reason is that:

[0215] Comparative Example 2 adopts a process flow of hydrogenation followed by cutting, and uses a conventional hydrogenation catalyst to treat the reforming raffinate oil. Due to the slightly poor hydrogenation performance of the catalyst, the removal rates of olefins and benzene are low. The C5 component cannot meet the standard requirements of the bromine index of the pentane foaming agent due to the presence of olefins, and the C7 and above components cannot meet the requirements of the sulfur content of 120# solvent oil due to the lack of removal of cyclopentane sulfone. At the same time, since the isohexane normalization reaction unit is not set up, isohexane cannot be converted into normal-hexane, which reduces the yield of normal-hexane and fails to achieve efficient utilization of the reforming raffinate oil.

[0216] In contrast, Examples 2a to 2e use the process flow of the present invention to treat the reforming raffinate oil, and achieve efficient utilization of the reforming raffinate oil by adding an adsorption desulfurization unit and a normalization reaction unit.

[0217] Among them, Examples 2a to 2c can achieve regulation of the purity and yield of n-hexane by adjusting the operating temperature of the top and bottom of the distillation tower; Examples 2b and 2d can achieve different degrees of removal of benzene and olefins by changing the operating temperature of the hydrogenation catalyst. In contrast, the operating temperature of the hydrogenation catalyst in Comparative Example 1 did not reach 90°C-200°C, and the removal of benzene and olefins was not complete; Examples 2b and 2e can achieve different degrees of normalization of isohexane to generate n-hexane and adjust the purity of n-hexane by changing the normalization reaction conditions.

[0218] The above results indicate that the method for producing solvent oil from reforming raffinate oil provided by the present invention is suitable for the separation and utilization of reforming raffinate oil with relatively high benzene and olefin contents, and the produced solvent oil has high purity and yield, good utilization effect, and can effectively improve the added value of reforming raffinate oil.

Claims

1. A method for preparing a hydrogenation catalyst, wherein: The preparation method comprises: The temperature of the carrier precursor slurry reaches the precipitation reaction temperature, and the pH value of the carrier precursor slurry is adjusted to an alkaline pH value to obtain a first mixed system; Adding a first active metal component precursor, a second active metal component precursor, and a precipitant to the first mixed system in parallel, maintaining the pH of the system at an alkaline pH value, to obtain a second mixed system; Performing an aging treatment on the second mixed system, and calcining the aging product to obtain the hydrogenation catalyst; The hydrogenation catalyst comprises a carrier and a first active metal component and a second active metal component supported on the carrier, wherein the metal element of the first active metal component comprises nickel. Based on the total weight of the catalyst being 100%, the weight content of the first active metal component in the catalyst is 40-70%, the weight content of the carrier in the catalyst is 20-59%, and the remainder is the second active metal component.

2. The preparation method according to claim 1, wherein The alkaline pH value is 8-11.

3. The preparation method according to claim 1, wherein The precipitation reaction temperature is 40-90°C.

4. The preparation method according to claim 1, wherein The temperature of the aging treatment is 40-90°C.

5. The preparation method according to claim 1, wherein The calcination temperature is 300-600°C.

6. The method for preparing a hydrogenation catalyst according to claim 1, wherein: The first active metal component precursor is a compound of the metal element in the first active metal component; The second active metal component precursor is a compound of the metal element in the second active metal component; The precipitant includes an alkaline precipitant.

7. The method for preparing a hydrogenation catalyst according to claim 6, wherein: The first active metal component precursor includes a metal salt of a metal element in the first active metal component.

8. The method for preparing a hydrogenation catalyst according to claim 6, wherein: The second active metal component precursor includes a metal salt of a metal element in the second active metal component.

9. The method for preparing a hydrogenation catalyst according to claim 6, wherein: The precipitating agent includes a soluble carbonate salt.

10. A hydrogenation catalyst obtained by the preparation method of the hydrogenation catalyst according to any one of claims 1 to 9.

11. The hydrogenation catalyst according to claim 10, wherein The dispersion degree of Ni metal in the hydrogenation catalyst is above 10%; The metal element of the second active metal component includes one or a combination of two or more of copper, lanthanum and magnesium; The carrier includes one of aluminum oxide, silicon oxide, titanium oxide, and cerium oxide, and / or a mixture of aluminum oxide and at least one of silicon oxide, titanium oxide, and cerium oxide.

12. The hydrogenation catalyst according to claim 10, wherein The specific surface area of ​​the hydrogenation catalyst is 200-500m 2 / g, the pore volume of the hydrogenation catalyst is 0.3-0.6cm 3 / g.

13. A method for producing solvent oil by reforming raffinate oil, the method comprising: S2, using a hydrogenation catalyst to catalyze the desulfurized and dehydrated reforming raffinate oil to perform a hydrogenation debenzenization and deolefination reaction to obtain a reaction product; S3, performing gas-liquid separation on the reaction product obtained in S2; S4, distilling the separated liquid to respectively distill out C5 component, C6 component and components above C7; S5, distilling the C6 component to respectively distill out cyclohexane and a mixture of normal hexane and isohexane; S6, distilling the mixture of normal hexane and isohexane to respectively distill out isohexane and normal hexane, thereby completing the production of solvent oil; Wherein, the hydrogenation catalyst comprises the hydrogenation catalyst according to any one of claims 10-12.

14. The method according to claim 13, wherein: In S2, the conditions for the hydrodebenzenization and deolefination reactions are: temperature 90-200°C, reaction pressure 1.0-3.0 MPa, hydrogen-oil volume ratio 100-300:1, volume space velocity 1.0-3.0 h -1 ; In S4, the distillation pressure is 0-0.2MPa; In S5, the distillation pressure is 0-0.1 MPa; In S6, the distillation pressure is 0-0.1 MPa.

15. The method according to claim 14, wherein: In S2, the reaction product has a benzene content of ≤0.01% and a bromine index of ≤50 mgBr / 100 g.

16. The method according to claim 14, wherein: The distillation process of S4 is completed in a distillation tower, the top temperature of the distillation tower is 30-50°C, and the bottom temperature of the tower is 90-110°C.

17. The method according to claim 14, wherein: The distillation process of S5 is completed in a distillation tower, and the top temperature of the distillation tower is 55-75°C and the bottom temperature of the tower is 70-90°C.

18. The method according to claim 14, wherein: The distillation process of S6 is completed in a distillation tower, and the top temperature of the distillation tower is 50-70°C and the bottom temperature of the tower is 60-80°C.

19. The method according to claim 13, wherein: In the reforming raffinate oil that has not been desulfurized and dehydrated, the sulfur content is below 20 mg / kg, the benzene content is 3-5v%, the olefin content is 1-3v%, and the total content of n-hexane and isohexane is greater than 50v%.

20. The method according to claim 19, wherein: The method further comprises: S1, desulfurizing and dehydrating the reforming raffinate oil, and the product S is ≤1 mg / kg.

21. The method according to claim 20, wherein: In S1, the space velocity during the desulfurization and dehydration process is 1-10h -1 .

22. The method according to claim 20, wherein: In S1, the adsorbent used for desulfurization and dehydration includes a molecular sieve adsorbent.

23. The method according to claim 22, wherein: The molecular sieve adsorbent includes one or a combination of two or more of 3A molecular sieve, 4A molecular sieve, 5A molecular sieve and 13A molecular sieve.

24. The method according to claim 22, wherein: The specific surface area of ​​the molecular sieve adsorbent is 400-700m 2 / g, pore volume is 0.05-0.30cm 3 / g.

25. The method according to any one of claims 13 to 24, wherein: The method further comprises: S7, converting the isohexane obtained in S6 into normal-hexane through a normalization reaction.

26. The method according to claim 25, wherein: The conditions of the normalization reaction are: reaction temperature 200-400°C, reaction pressure 1.0-3.0MPa, hydrogen-oil volume ratio 100-300:1, volume space velocity 1.0-3.0h -1 .

27. The method according to claim 25, wherein: The purity of the isohexane is above 90%.

28. The method according to claim 27, wherein: The purity of the isohexane is above 95%.

29. The method according to claim 25, wherein: The catalyst for the normalization reaction comprises a molecular sieve catalyst, which comprises a third active metal component, a molecular sieve support and a non-molecular sieve support.

30. The method of claim 29, wherein: The molecular sieve carrier includes one or a combination of two or more of MOR, MCM-41, ZSM-22 and SAPO-11.

31. The method of claim 29, wherein: The metal elements in the third active metal component include elements in Group VIB and / or Group VIII.

32. The method of claim 29, wherein: The non-molecular sieve support comprises alumina.

33. The method of claim 29, wherein: Taking the total weight of the molecular sieve catalyst as 100%, the weight of the molecular sieve carrier accounts for 10-80% of the total weight of the catalyst, the weight of the third active metal component accounts for 0.01-5% of the total weight of the catalyst, and the remainder is non-metallic carrier.

34. The method of claim 33, wherein: Based on the total weight of the molecular sieve catalyst being 100%, the weight of the third active metal component accounts for 0.1-0.5% of the total weight of the catalyst.

35. The method of claim 33, wherein: The weight of the third active metal component accounts for 0.1-0.5% of the total weight of the catalyst.

36. A system for producing solvent oil by reforming raffinate oil, wherein the system is capable of implementing the method for producing solvent oil by reforming raffinate oil as claimed in any one of claims 13 to 35.

37. The system for producing solvent oil from reformed raffinate oil according to claim 36, wherein: The system for producing solvent oil by reforming raffinate oil comprises a desorption desulfurization reactor, a hydrogenation reactor, a gas-liquid separator, a first distillation tower, a second distillation tower, and a third distillation tower which are connected in sequence.

38. The system for producing solvent oil from reformed raffinate oil according to claim 37, wherein: The system for producing solvent oil by reforming raffinate oil also includes a normalization reactor and a gas-liquid separator, wherein the inlet of the normalization reactor is connected to the outlet of the third distillation tower, and the outlet of the normalization reactor is connected to the inlet of the gas-liquid separator.