Thermally conductive sheets and their manufacturing methods
By controlling the ratio of addition-curing silicone polymers and unreacted silicone oils to mix with thermally conductive inorganic particles, thermally conductive sheets are prepared, solving the problems of low thermal conductivity and oil seepage, achieving the effect of high thermal conductivity and low oil seepage, which is suitable for improving the heat dissipation of electrical and electronic components.
Patent Information
- Application Number
- CN202180072624.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-12-16
- Filing Date
- 2021-07-01
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2041-07-01
AI Technical Summary
Existing thermally conductive silicone compositions suffer from low thermal conductivity and oil seepage problems.
A thermally conductive sheet is formed by preparing a thermally conductive sheet containing an addition-curing silicone polymer and unreacted silicone oil, controlling the ratio of the two, mixing it with thermally conductive inorganic particles, and then forming and curing the sheet.
It improves thermal conductivity, inhibits oil seepage, and reduces compressive load, making it suitable for improving heat dissipation of electrical and electronic components.
Smart Images

Figure CN116419951B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a thermally conductive sheet suitable for sandwiching between a heat-generating part and a heat sink in electrical or electronic components, and a method for manufacturing the same. Background Technology
[0002] The performance improvements of semiconductors such as CPUs in recent years have been remarkable, but this has also led to a surge in heat generation. Therefore, heat sinks are installed in heat-generating electronic components, and thermally conductive silicone gels are used to improve the adhesion between the semiconductor and the heat sink. Previous methods of creating gel-like cured thermally conductive silicones achieved this by creating an imbalance in the ratio of alkenyl to Si-H groups in the composition, leaving unreacted portions. However, if an imbalance in the alkenyl to Si-H group ratio is used to create a gel-like cured product, unreacted oil from the raw materials remains in the cured product, causing oil seepage.
[0003] Patent Document 1 discloses a heat dissipation material comprising an organopolysiloxane having at least one alkenyl group bonded to a silicon atom in one molecule, an organohydrogen polysiloxane having at least two hydrogen atoms bonded to a silicon atom in one molecule, a platinum-based catalyst, and thermally conductive particles. Claim 3 specifies the use of an organohydrogen polysiloxane with a high Si-H group. Patent Document 2 discloses the use of an alkenyl-containing polyorganosiloxane with a specific viscosity and a diorganohydrosiloxy-terminated polyorganosiloxane to produce a gel with low oil exudation. The polyorganosiloxane has an average of about two alkenyl groups bonded to a silicon atom in one molecule, and the other organic groups bonded to the silicon atom are substituted or unsubstituted monovalent hydrocarbon groups without aliphatic unsaturated bonds. Patent Document 3 discloses surface treatment of the thermally conductive particles.
[0004] Existing technical documents
[0005] Patent documents
[0006] Patent Document 1: Japanese Patent Application Publication No. 2005-344106
[0007] Patent Document 2: Japanese Patent Application Publication No. 2008-143980
[0008] Patent Document 3: Japanese Patent Application Publication No. 2020-002236 Summary of the Invention
[0009] The problem that the invention aims to solve
[0010] However, conventional thermally conductive silicone compositions suffer from low thermal conductivity.
[0011] In order to solve the above-mentioned problems, the present invention provides a thermally conductive sheet with high thermal conductivity and suppresses oil seepage, and a method for manufacturing the same.
[0012] Methods for solving problems
[0013] The thermally conductive sheet of the present invention is characterized in that it comprises a matrix resin (A) and thermally conductive inorganic particles (B), wherein the matrix resin (A) comprises an addition-curing silicone polymer (A1) and unreacted silicone oil (A2), wherein when the matrix resin (A) is set to 100% by mass, the addition-curing silicone polymer (A1) is 20% by mass or more and less than 100% by mass, the unreacted silicone oil (A2) is more than 0% by mass and less than 80% by mass, and the thermally conductive inorganic particles (B) are 1000 to 3000 parts by mass relative to 100 parts by mass of the matrix resin (A), and the thermally conductive sheet is cured.
[0014] The method for manufacturing the thermally conductive sheet of the present invention is characterized in that it is a method for manufacturing a thermally conductive sheet comprising an addition-cured silicone polymer (A1), unreacted silicone oil (A2), and thermally conductive inorganic particles.
[0015] The aforementioned matrix resin (A) comprises an addition-curing silicone polymer (A1) and an unreacted silicone oil (A2).
[0016] When the matrix resin (A) is set to 100% by mass, the addition-curing silicone polymer (A1) is 20% by mass or more and less than 100% by mass, and the unreacted silicone oil (A2) is more than 0% by mass and less than 80% by mass.
[0017] Relative to 100 parts by mass of the matrix resin (A), the thermally conductive inorganic particles (B) are 1000 to 3000 parts by mass.
[0018] The components comprising the above-mentioned addition-curing silicone polymer (A1), the above-mentioned unreacted silicone oil (A2), and the above-mentioned thermally conductive inorganic particles (B) are mixed, formed into a sheet, and cured.
[0019] Invention Effects
[0020] The thermally conductive sheet of the present invention comprises a matrix resin (A) and thermally conductive inorganic particles (B). The matrix resin (A) comprises an addition-curing silicone polymer (A1) and unreacted silicone oil (A2). When the matrix resin (A) is set to 100% by mass, the addition-curing silicone polymer (A1) is 20% by mass or more and less than 100% by mass, the unreacted silicone oil (A2) is more than 0% by mass and less than 80% by mass, and the thermally conductive inorganic particles (B) are 1000 to 3000 parts by mass relative to 100 parts by mass of the matrix resin (A). The thermally conductive sheet is cured, thereby providing a thermally conductive sheet with high thermal conductivity and a method for manufacturing the same. Furthermore, by partially replacing the addition-curing silicone polymer (A1) with unreacted silicone oil (A2), the present invention can provide a thermally conductive silicone composition that inhibits oil seepage. Furthermore, the crosslinking density is relatively lower compared to addition-cured silicone polymers alone, which can suppress compressive loads to a lower level. Attached Figure Description
[0021] Figure 1A -B is an explanatory diagram illustrating a method for measuring the thermal conductivity of a sample in one embodiment of the present invention.
[0022] Figure 2A This is a schematic cross-sectional view illustrating an oil seepage width measurement test in one embodiment of the present invention. Figure 2B It is a schematic plan view for measuring the width of the oil seepage. Detailed Implementation
[0023] This invention relates to a thermally conductive sheet comprising a matrix resin (A) and thermally conductive inorganic particles (B). The matrix resin (A) comprises an addition-curing silicone polymer (A1) and unreacted silicone oil (A2). When the matrix resin (A) is set to 100% by mass, the addition-curing silicone polymer (A1) is 20% by mass or more and less than 100% by mass, and the unreacted silicone oil (A2) is more than 0% by mass and less than 80% by mass. Preferably, the addition-curing silicone polymer (A1) is 30% by mass or more and less than 90% by mass, and the unreacted silicone oil (A2) is 10% by mass or more and less than 70% by mass. If these ranges are met, oil exudation is suppressed to a lower degree.
[0024] The thermally conductive inorganic particles (B) are 1000 to 3000 parts by mass relative to 100 parts by mass of the matrix resin (A), preferably 1500 to 2200 parts by mass. If the content falls within the above range, the thermal conductivity can be improved.
[0025] The viscosity of the unreacted silicone oil (A2) at 25°C is preferably 50–3000 mm. 2 / s, more preferably 70 to 2500 mm 2 / s. Viscosity was measured using a Brookfield Sp No.2 rotational viscometer. If the viscosity is within the above range, oil seepage is suppressed to a low degree, and the filling of thermally conductive inorganic particles is also good. Unreacted silicone oils are dimethylpolysiloxane, diphenylpolysiloxane, etc., which are silicone polymers without reactive groups.
[0026] The thermal conductivity of the thermally conductive sheet is preferably 5.0–15.0 W / mK, more preferably 6.0–15.0 W / mK, and even more preferably 7.0–15.0 W / mK. Thermal conductivity within this range is useful for many devices.
[0027] A thermally conductive sheet is 25 mm long, 25 mm wide, and 1 mm thick, sandwiched between a glass plate and pharmaceutical paper, with a compression rate of 50%. When held at 125°C for 72 hours, the oil seepage width is preferably 9.5 mm or less. More preferably, the oil seepage width is 3 mm or less. This allows for significantly reduced oil seepage.
[0028] The 50% compressive load value of the thermally conductive sheet of the present invention is preferably 1000 N or less, more preferably 600 N or less. This makes it easy to crush, thus reducing the physical load on the heating element.
[0029] The method for manufacturing the thermally conductive sheet of the present invention is as follows.
[0030] (1) As the matrix resin (A), an addition-curing silicone polymer (A1) and an unreacted silicone oil (A2) are prepared. When the matrix resin (A) is set to 100% by mass, the addition-curing silicone polymer (A1) is 20% by mass or more and less than 100% by mass, and the unreacted silicone oil (A2) is set to more than 0% by mass and less than 80% by mass. In addition, the thermally conductive inorganic particles (B) are set to 1000 to 3000 parts by mass relative to 100 parts by mass of the matrix resin (A).
[0031] As the aforementioned addition-curing silicone polymer (A1), the following silicone polymer is preferably used: a silicone polymer in which a cured sheet of a composition in which 1000 to 3000 parts by mass of thermally conductive inorganic particles are added to 100 parts by mass of the addition-curing silicone polymer is set to a length of 25 mm, a width of 25 mm, and a thickness of 1 mm, sandwiched between a glass plate and pharmaceutical paper, with a compression ratio set to 50%, has an oil permeation width of 1.5 mm or less when held at 125°C for 72 hours. Thus, the oil permeation width of the cured thermally conductive sheet is also suppressed to a low level. Hereinafter, the oil permeation width of the cured sheet composed of the addition-curing silicone polymer and the thermally conductive inorganic particles will be referred to as the oil permeation width of the cured sheet of the base polymer composition.
[0032] (2) The components comprising addition-curing silicone polymer (A1), unreacted silicone oil (A2), and thermally conductive inorganic particles (B) are mixed, formed into a sheet, and cured. Mixing is preferably performed using a kneader, homogenizer, planetary mixer, or dissolver. Degassing under reduced pressure is preferably performed during or after mixing. The sheet is formed to a specified thickness using rolling, pressing, or similar methods. Curing can be performed at room temperature or by heat curing. In the case of heat curing, a heat treatment is performed at 80–120°C for 5–40 minutes.
[0033] The thermally conductive inorganic particles are preferably selected from at least one inorganic particle chosen from alumina, zinc oxide, silicon oxide, silicon carbide, aluminum nitride, boron nitride, aluminum hydroxide, and silicon dioxide. Alumina and aluminum nitride are particularly preferred. The shape of the thermally conductive inorganic particles is spherical, irregular, needle-like, plate-like, etc., without particular limitation.
[0034] As alumina, there are various types, including spherical alumina produced by heating and melting, sintered alumina produced by furnace firing, fused alumina produced by electric arc furnace melting, and high-purity alumina produced by methods such as hydrolysis of aluminum alkoxides or in-situ chemical vapor deposition, and there are no particular limitations. The obtained alumina particles can also be set to a target particle size range by crushing or the like. Thus, fragmented alumina particles can be obtained. In this invention, fragmented alumina particles are preferred.
[0035] Aluminum nitride includes known forms produced by direct nitriding, reduction nitriding, combustion synthesis, etc., as well as agglomerated aluminum nitride obtained by further agglomerating the obtained aluminum nitride, and there is no particular limitation. The obtained aluminum nitride particles can also be set to a target particle size range by crushing, etc. Thus, fragmented aluminum nitride particles can be obtained. In this invention, fragmented aluminum nitride particles are preferred.
[0036] The average particle size of the thermally conductive inorganic particles is preferably 0.01 μm or more and 200 μm or less, more preferably 0.1 μm or more and 150 μm or less. It should be noted that the average particle size is the D50 (median particle size) of the cumulative particle size distribution based on volume in particle size distribution determination using laser diffraction light scattering method.
[0037] The matrix resin used above is an addition-curing silicone polymer (organopolysiloxane). This polymer has high heat resistance and is useful for making thermally conductive sheets. Commercially available organopolysiloxanes can be used, with a preferred viscosity of 100–10000 mPa·s. The addition-curing silicone polymer (organopolysiloxane) is cured via an addition reaction using a platinum-based curing catalyst. Typically, it is separated into liquid A and liquid B, one liquid containing a platinum-based curing catalyst and the other liquid containing a vulcanizing agent (curing agent). The two liquids are mixed to form a composition, which is then cured after sheet forming.
[0038] Thermally conductive sheets can also be further supplemented with more than 0 parts by weight and less than 200 parts by weight of a silane coupling agent relative to 100 parts by weight of the matrix resin. One example of a silane coupling agent is R-Si(CH3). a (OR') 4-a The silane compound or its partial hydrolysate represented by the formula (where R is a non-substituted or substituted organic group having 1 to 20 carbon atoms, R' is an alkyl group having 1 to 4 carbon atoms, and a is 0 or 1) is included. Examples of alkoxysilane compounds (hereinafter referred to as "silanes") represented by the above chemical formula include methyltrimethoxysilane, ethyltrimethoxysilane, propyltrimethoxysilane, butyltrimethoxysilane, pentyltrimethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, octyltrimethoxysilane, octyltriethoxysilane, decylmethoxysilane, decyltriethoxysilane, dodecyltrimethoxysilane, dodecyltriethoxysilane, hexa(dodecyl)trimethoxysilane, hexa(dodecyl)triethoxysilane, octadecyltrimethoxysilane, and octadecyltriethoxysilane. One or more of the above silane compounds may be used. Silane coupling agents can be used as surface treatment agents for thermally conductive inorganic particles.
[0039] In the thermally conductive sheet of the present invention, other components besides those mentioned above can be added as needed. For example, heat-resistant improvers such as iron oxide red, titanium oxide, and cerium oxide, flame retardants, and curing delay agents can also be added. Organic or inorganic pigments can also be added for coloring and tinting purposes. The silane coupling agent mentioned above can also be added.
[0040] Example
[0041] The following examples are used for illustration. This invention is not limited to these examples. Various parameters were measured using the methods described below.
[0042] Thermal conductivity
[0043] The thermal conductivity of thermally conductive greases is determined using a Hot Disk (according to ISO / CD 22007-2). This thermal conductivity measuring apparatus 1 is as follows: Figure 1A As shown, the polyimide film sensor 2 is clamped between two samples 3a and 3b. A constant power is applied to the sensor 2, causing it to heat up constantly, and the thermal characteristics are analyzed based on the temperature rise of the sensor 2. The diameter of the front end 4 of the sensor 2 is 7 mm. Figure 1B As shown, the electrode has a double-helix structure, with an electrode 5 for applying current and an electrode 6 for measuring resistance (temperature measurement) arranged at the bottom. The thermal conductivity is calculated using the following formula (Mathematical Formula 1).
[0044] [Mathematical Expression 1]
[0045]
[0046] λ: Thermal conductivity (W / m·K)
[0047] P0: Constant power (W)
[0048] r: Radius of the sensor (m)
[0049] τ:
[0050] α: Thermal diffusivity of the sample (m) 2 / s)
[0051] t: Measurement time (s)
[0052] D(τ): A dimensionless function of τ
[0053] ΔT(τ): Temperature rise of the sensor (K)
[0054] <Method for determining the width of oil penetration>
[0055] Figure 2A This is a schematic cross-sectional view of the oil seepage width measuring test apparatus 11 in one embodiment of the present invention. The thermally conductive cured sheet sample 12 is set with a length of 25 mm, a width of 25 mm, and a thickness of 1 mm. It is clamped by two sheets of medicine wrapping paper 13 on an aluminum plate 14 and a glass plate 15 from above. The compression rate is set to 50%, and the oil seepage width (expansion) is measured at 125°C for 72 hours. Figure 2B This is a schematic plan view for measuring the width (expansion) of the oil seepage. The compressed size of the thermally conductive cured sheet sample 12 on the medicine packaging paper 13 is set as D2, and the length of the oil seepage area 16 from end to end is set as D1. The following formula is used to calculate the width (expansion) of the oil seepage area 16.
[0056] Oil seepage width = (D1 - D2) / 2
[0057] The unit is mm. The oil penetration width of the cured sheet of the base polymer composition was also measured in the same way.
[0058] Viscosity of unreacted silicone oil
[0059] Viscosity was measured using a Brookfield Sp No.2 rotational viscometer at 25°C.
[0060] <50% compressive load value>
[0061] Using the method according to ASTM D575-91:2012, a sample prepared with a diameter (φ) of 28.6 mm × 1.0 mm was clamped in an aluminum block of φ28.6 mm × 4.0 mm, and the instantaneous value was read when the sample was compressed to 50%.
[0062] (Examples 1-4, Comparative Example 1)
[0063] (1) Raw material composition
[0064] • Matrix resin (A)
[0065] As an addition-curing silicone polymer (A1), a commercially available two-component organopolysiloxane is used. One component contains a platinum-based curing catalyst, and the other component contains a vulcanizing agent (curing agent).
[0066] As the unreacted silicone oil (A2), commercially available dimethyl silicone oil (viscosity: 100 mm) was used. 2 / s).
[0067] • Thermally conductive inorganic particles (B): Aluminum nitride (average particle sizes of 70 μm, 20 μm, and 1 μm, with fragmented particle shape) and alumina (average particle size of 0.3 μm, with fragmented particle shape) were added in a ratio of 1500 parts by mass relative to 100 parts by mass of the matrix resin (A). The alumina filler used was alumina filler that had undergone surface treatment (pretreatment) with n-octyltriethoxysilane. The surface treatment involved adding 2.48 parts by mass of n-octyltriethoxysilane relative to 100 parts by mass of alumina, stirring, and then heating at 125°C for 12 hours.
[0068] (2) Mixing
[0069] Add the above raw materials to a planetary mixer and mix at 23°C for 10 minutes. Degas under reduced pressure during or after mixing.
[0070] (3) Forming of cured sheets
[0071] The mixed thermally conductive composition is rolled to a thickness of 1 mm to form a sheet, which is then placed in an oven at 100°C for 20 minutes for heat curing.
[0072] The various physical properties of the obtained cured sheets are summarized in Table 1. In Table 1, "Oil penetration width of the base polymer composition" refers to the oil penetration width of the cured sheet without silicone oil. Furthermore, the oil penetration width of the cured sheet with silicone oil is simply expressed as "oil penetration width." The same applies to Tables 2-4.
[0073] surface
[0074]
[0075] As shown in Table 1, the oil seepage width of Examples 1-4 was smaller than that of Comparative Example 1.
[0076] (Examples 5-8, Comparative Examples 2-3)
[0077] The thermally conductive inorganic particles (B) were set to a total of 2010 parts by mass relative to 100 parts by mass of the matrix resin (A), and the oil ratio was changed. Otherwise, the procedure was carried out in the same manner as in Example 1. The conditions and results are shown in Table 2.
[0078] Table 2
[0079]
[0080] As shown in Table 2, Examples 5-8 exhibited smaller oil exudation widths compared to Comparative Example 3. Furthermore, regarding the 50% compressive load value, Examples 5-8 were lower than Comparative Example 2. This is because the crosslinking density is relatively lower compared to that of the addition-cured silicone polymer alone.
[0081] (Examples 9-11)
[0082] The thermally conductive inorganic particles (B) were set to a total of 2200 parts by mass relative to the matrix resin (A) at 100 parts by mass, and the oil ratio was changed. Otherwise, the procedure was carried out in the same manner as in Example 1. The conditions and results are shown in Table 3.
[0083] Table 3
[0084]
[0085] As shown in Table 3, the oil seepage width of Examples 9-11 is small.
[0086] (Comparative Examples 4-9)
[0087] The oil exudation widths of the base polymer compositions are shown in Table 4 for the addition-curing silicone polymer (A1), with variations in the oil ratio, otherwise performed in the same manner as in Example 1. The conditions and results are shown in Table 4.
[0088] Table 4
[0089]
[0090] As shown in Table 4, Comparative Examples 4-9 are not preferred because the oil penetration width of the base polymer composition is high, and therefore the oil penetration width of the thermally conductive cured sheet is also high.
[0091] Industrial availability
[0092] The thermally conductive silicone sheet of the present invention is suitable for being sandwiched between the heat-generating part of electrical or electronic components and a heat sink.
[0093] Explanation of symbols
[0094] 1 Thermal conductivity measuring device
[0095] 2 sensors
[0096] Samples 3a and 3b
[0097] 4. Front end of the sensor
[0098] 5. Electrodes for applying current
[0099] 6. Electrodes for resistance measurement (electrodes for temperature measurement)
[0100] 11. Test apparatus for measuring oil seepage width
[0101] 12 Thermally conductive cured sheet samples
[0102] 13 packs of medicine paper
[0103] 14 Aluminum Plate
[0104] 15 Glass Plates
[0105] 16 Oil seepage area
Claims
1. A thermally conductive sheet comprising a matrix resin (A) and thermally conductive inorganic particles (B), The matrix resin (A) comprises an addition-curing silicone polymer (A1) and an unreacted silicone oil (A2). When the matrix resin (A) is set to 100% by mass, the addition-curing silicone polymer (A1) is 20% by mass or more but less than 100% by mass, and the unreacted silicone oil (A2) is more than 0% by mass but less than 80% by mass. The thermally conductive inorganic particles (B) are 1000 to 3000 parts by mass relative to 100 parts by mass of the matrix resin (A). The thermally conductive inorganic particles include fragmented alumina particles and fragmented aluminum nitride particles. The thermally conductive sheet is cured. A cured sheet of a base polymer composition containing 1,000 to 3,000 parts by weight of thermally conductive inorganic particles (B) added to 100 parts by weight of the addition-curing silicone polymer (A1) and free of unreacted silicone oil (A2) is configured to have a length of 25 mm, a width of 25 mm, and a thickness of 1 mm. The sheet is sandwiched between a glass plate and pharmaceutical paper and the compression ratio is set to 50%. When the sheet is kept at 125°C for 72 hours, the oil seepage width is less than 1.5 mm.
2. The thermally conductive sheet according to claim 1, wherein, The unreacted silicone oil (A2) has a viscosity of 50–3000 mm at 25°C. 2 / s.
3. The thermally conductive sheet according to claim 1 or 2, wherein, The thermal conductivity of the thermally conductive sheet is 5.0 to 15.0 W / mK.
4. The thermally conductive sheet according to claim 1 or 2, wherein, The cured thermally conductive sheet is set to a length of 25 mm, a width of 25 mm, and a thickness of 1 mm. It is sandwiched between a glass plate and a medicine wrapping paper, and the compression rate is set to 50%. When kept at 125°C for 72 hours, the oil seepage width is less than 9.5 mm.
5. The thermally conductive sheet according to claim 1 or 2, wherein, The thermally conductive inorganic particles further include other thermally conductive inorganic particles, which are at least one inorganic particle selected from the group consisting of aluminum oxide, zinc oxide, silicon oxide, silicon carbide (excluding fragmented forms), aluminum nitride, boron nitride, aluminum hydroxide, and silicon dioxide (excluding fragmented forms).
6. The thermally conductive sheet according to claim 1 or 2, wherein, The thermally conductive sheet has a 50% compressive load value of less than 1000N.
7. The thermally conductive sheet according to claim 1 or 2, wherein, The average particle size of the thermally conductive inorganic particles is greater than 0.01 μm and less than 200 μm.
8. A method for manufacturing a thermally conductive sheet, characterized in that, It is a method for manufacturing a thermally conductive sheet comprising any one of claims 1 to 7, including a matrix resin (A) and thermally conductive inorganic particles (B). The matrix resin (A) comprises an addition-curing silicone polymer (A1) and an unreacted silicone oil (A2). When the matrix resin (A) is set to 100% by mass, the addition-curing silicone polymer (A1) is 20% by mass or more but less than 100% by mass, and the unreacted silicone oil (A2) is more than 0% by mass but less than 80% by mass. The thermally conductive inorganic particles (B) are 1000 to 3000 parts by mass relative to 100 parts by mass of the matrix resin (A). The thermally conductive inorganic particles include fragmented alumina particles and fragmented aluminum nitride particles. The components comprising the addition-curing silicone polymer (A1), the unreacted silicone oil (A2), and the thermally conductive inorganic particles (B) are mixed, formed into a sheet, and then cured.
Citation Information
Patent Citations
Silicone gel composition
JP2005344106A
Composition for heat radiation silicone gel and heat radiation silicone sheet obtained by curing the same
JP2008143980A
Heat-conductive silicone composition, heat-conductive silicone sheet, and method of manufacturing the same
JP2020002236A
Cured product of thermally conductive silicone composition
CN113166542A
Heat-resistant thermally conductive composition and heat-resistant thermally conductive sheet
JP6778846B1