Bagasse cellulose aerogel and preparation method thereof
Through the acid-base immersion etching method and normal pressure drying method of bagasse cellulose aerogel, combined with chitosan and glutaraldehyde, the problem of insufficient drying technology in the production of cellulose aerogel was solved and high porosity was achieved. The combination of strength and strength makes it suitable for thermal insulation and energy storage fields.
Patent Information
- Application Number
- CN202310478630.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-04-28
AI Technical Summary
The existing drying technology for cellulose aerogel production does not meet the demand, and it is difficult to ensure high porosity and strength at the same time. Moreover, the traditional method has expensive equipment, long cycle time, and high cost, which limits large-scale production and application.
Sugarcane bagasse is used as raw material, cellulose is extracted through acid-base soaking and etching method, and chitosan and glutaraldehyde are used as reinforcing agents and cross-linking agents, combined with normal pressure drying method, to prepare low density, good hydrophobicity and barrier properties. Sugarcane bagasse cellulose aerogel with excellent combustion performance.
Industrialized production with simple process, low cost, short cycle and low equipment requirements has been achieved, and bagasse cellulose aerogels with low density, high porosity and high strength have been prepared, which are suitable for fields such as thermal insulation and energy storage.
Smart Images

Figure CN116426032B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of cellulose aerogels and specifically relates to bagasse cellulose aerogel and a preparation method thereof. Background Art
[0002] Aerogels have high porosity (>95%) and low density (3–150 mg / cm 3 ), low thermal conductivity and large specific surface area (500–1000m 2 / g) and many other advantages, and can be applied to various fields, including thermal insulation, pollutant treatment, electromagnetic shielding, sensors, catalysis and energy storage, etc., and are ideal thermal insulation materials. At present, most aerogel materials, such as traditional aerogels such as silica aerogels, have been commercially applied, but they have disadvantages such as poor toughness, difficulty in molding and high cost; organic polymer aerogels have the advantages of excellent flexibility, easy processing and low cost, but they are mostly prepared with non-renewable and non-degradable materials, and their difficult degradation and high pollution limit their wide application.
[0003] Cellulose is a macromolecular polysaccharide composed of glucose. It is abundant in nature and is green, pollution-free, renewable and sustainable. It also contains abundant active hydroxyl groups and can undergo cross-linking reactions with water or other cross-linking agents to form hydrogels with three-dimensional network structures. It is an excellent material for making aerogels. However, the production of cellulose aerogels does not meet the drying technology requirements, and it is difficult for cellulose aerogels to have high strength while ensuring their high porosity, so large-scale production and application are not possible.
[0004] Han [Han ZM, Sun WB, Yang KP, et al. An all-natural wood-inspired aerogel [J]. Angew Chem Int Ed Engl, 2022.] et al. used poplar wood powder as raw material, montmorillonite and sodium alginate as additives, and calcium chloride solution as a cross-linking agent to prepare lightweight and porous cellulose aerogel by freeze drying. However, this method uses a freeze drying process to prepare aerogels, which has a complicated process, expensive equipment, a long cycle, and a limited size of the prepared product, which limits its practical application.
[0005] Ma et al. (Ma ZH, Han Y, et al. Highly efficient oil–water separation of superhydrophobic cellulose II aerogel based on dissolution and regeneration of cotton in lithium bromide system [J]. Journal of Molecular Liquids, 2022, 367: 120543.) used cotton as raw material and LiBr solution as solvent, and prepared lightweight and porous cellulose aerogel by freeze drying. However, the mechanical properties of the prepared cellulose aerogel are poor, and its compressive stress is only 113.2 kPa when the deformation is 80%; and the freeze drying method has high preparation cost and long cycle, and it is difficult to prepare large-size samples.
[0006] Chang Huanjun et al. (Chang Huanjun, Zhang Longfei et al. Effects of two drying methods on the structure and properties of carbon nanotube / nanocellulose aerogels [J]. Wood Science and Technology, 2022, 36(5): 43-49.) First, carbon nanotubes and cellulose were used as raw materials, and cellulose aerogels were prepared by freeze drying and supercritical drying, respectively. The cellulose aerogel prepared by supercritical drying showed a filamentous porous structure, and its pore structure was mainly mesoporous. Compared with the freeze-dried sample, the specific surface area of the prepared cellulose aerogel increased by 5.6 times and the pore volume increased by 5.13 times. Although supercritical drying can maintain the mesoporous structure of cellulose aerogel to the greatest extent and prepare cellulose aerogels with excellent performance, the equipment used in the supercritical drying method is expensive, and the apparatus used is an autoclave, which has high requirements for airtightness; the process is cumbersome, and solvent exchange is required before the wet gel is dried; the experimental cycle is long, the output is low, and the cost is high, which is only suitable for preparing a small amount of high-performance products.
[0007] He [He S, Liu C, Chi X, et al. Bio-inspired lightweight pulp foams with improved mechanical property and flame retardancy viaborate cross-linking [J]. Chemical Engineering Journal, 2019, 371: 34-42.] et al. used bleached coniferous pulp as raw material, borax as cross-linking agent, sodium dodecyl sulfate as foaming agent, and successfully prepared cellulose aerogel by atmospheric pressure drying method. The sample has a compressive strength of 74.1 kPa (deformation is 50%), and the flame retardant and self-extinguishing properties are poor, but the sample has poor strength and cannot meet daily use.
[0008] Li et al. [Li Y, Grishkewich N, Liu L, et al. Construction of functional cellulose aerogels via atmospheric drying chemically cross-linked and solventexchanged cellulose nanofibrils [J]. Chemical Engineering Journal, 2019, 366: 531-538.] used glycyloxypropyltrimethoxysilane and branched polyethyleneimine to increase the connection strength between celluloses, and replaced the water in the gel with acetone to reduce the surface tension of the solvent. On the cellulose surface, the silanols produced by the hydrolysis of glycyloxypropyltrimethoxysilane cross-link with the hydroxyl groups. At the same time, strong interactions occur between the epoxide groups of glycyloxypropyltrimethoxysilane and the amine groups of branched polyethyleneimine, thereby increasing the cross-linking density of the gel network. The acetone solvent exchange method is used to replace the water inside the cellulose hydrogel with low surface energy substances, thereby achieving atmospheric pressure drying of the aerogel and saving preparation costs. Compared with freeze-dried samples, the cellulose aerogel dried at atmospheric pressure has a similar density (58.82 g / cm 3 ), 4.3 times the specific surface area (22.4m 2 / g) and similar compression resilience (50% deformation, 5 times compression and rebound without obvious permanent deformation). However, organic solvents have the disadvantage of being expensive. Summary of the invention
[0009] The present invention aims to overcome the deficiencies of the prior art and aims to provide a method for preparing bagasse cellulose aerogels of any size by a normal pressure drying method, which has the advantages of simple process, low cost, short cycle, low equipment requirements, easy industrial production, high added value utilization of bagasse and atmospheric pressure drying; the bagasse cellulose aerogels prepared by the method have low density, good hydrophobicity and excellent flame retardant properties, and especially have high porosity and high strength at the same time.
[0010] To achieve the above object, the technical solution adopted by the present invention is:
[0011] Step 1, drying the cleaned bagasse in an oven at 80-85° C. for 22-24 hours to obtain dried bagasse; then crushing the dried bagasse, washing it with deionized water for 3-5 times, and then drying it at 80-90° C. for 22-24 hours to obtain pretreated bagasse.
[0012] Step 2: adding chitosan powder to acetic acid solution at a concentration of 1.9-2.1 wt%, stirring at a speed of 300-600 rpm for 2-3 hours to obtain a chitosan solution.
[0013] Step 3: placing the pretreated bagasse in a sodium hydroxide solution at a mass ratio of 1:30 to 50, stirring the pretreated bagasse at a speed of 300 to 600 rpm for 0.8 to 1.2 h in a water bath at 80 to 85° C., and then washing with deionized water until neutral to obtain product A.
[0014] Step 4: placing the product A in a sodium chlorite solution at a mass ratio of 1:30-50 to the pretreated bagasse and the sodium chlorite solution, adjusting the pH to 4.5-5 with acetic acid; then moving the product A to a water bath at 80-85° C. and stirring at a speed of 300-600 rpm for 0.8-1.2 h, then washing the product A with deionized water until neutral, and drying the product A at 80-85° C. for 4-6 h to obtain cellulose.
[0015] Step 5: preparing a cellulose suspension by stirring the mixture at a speed of 300 to 600 rpm for 12 to 24 hours at a mass ratio of cellulose to deionized water of 1:95 to 97.
[0016] Step 6: Add the chitosan solution into the cellulose suspension, stir evenly, and prepare suspension B; the chitosan solution is 20-60 wt % of the cellulose suspension.
[0017] Step 7, according to the mass ratio of suspension B to glutaraldehyde aqueous solution of 1: 0.01-0.055, the suspension B is added to the glutaraldehyde aqueous solution, stirred at a speed of 300-600 rpm for 10-30 seconds, poured into a mold, and after gelling, placed at -20--18°C for 45-48 hours, taken out, and allowed to stand at room temperature for 12-24 hours, and then dried in an oven at 80-85°C for 20-24 hours to obtain bagasse cellulose aerogel.
[0018] The concentration of the acetic acid solution is 0.9-1.1 wt %.
[0019] The concentration of the sodium hydroxide solution is 2-3 wt %.
[0020] The concentration of the sodium chlorite solution is 2-3 wt %.
[0021] The glutaraldehyde content in the glutaraldehyde aqueous solution is 23-27 wt %.
[0022] Due to the adoption of the above technical solution, the present invention has the following positive effects and outstanding features compared with the prior art:
[0023] 1. The present invention uses bagasse as raw material and extracts bagasse cellulose through acid-base immersion etching method. The raw material source is wide and concentrated, realizing high added value utilization of bagasse, low cost and green environmental protection; and the cellulose has low density and is degradable, and the prepared bagasse cellulose aerogel has low density and is environmentally friendly.
[0024] 2. The present invention uses chitosan as a reinforcing agent to effectively enhance the connection strength between fibers and prevent fiber sliding, thereby improving the compression elasticity and compressive strength of the aerogel, and making the prepared bagasse cellulose aerogel have good hydrophobicity and flame retardancy.
[0025] 3. The present invention uses glutaraldehyde as a cross-linking agent, and its aldehyde groups are cross-linked with the amino groups of chitosan and the hydroxyl groups on the surface of cellulose to build a strong connection, thereby preventing the collapse of the aerogel structure during normal pressure drying, ensuring the structural stability of the bagasse cellulose aerogel, and thus improving the compressive elasticity and mechanical properties of the bagasse cellulose aerogel.
[0026] 4. The present invention adopts an aging method in a freezing environment to effectively prevent the evaporation of water in the gel, which not only makes the prepared bagasse cellulose aerogel have a higher porosity and a lower thermal conductivity, but also significantly shortens the preparation cycle.
[0027] 5. The present invention adopts the atmospheric pressure drying method to prepare cellulose aerogel. By adopting a more solid cross-linking method and increasing the pore size of the cellulose wet gel, the purpose of strengthening the connection between the cellulose networks and reducing the capillary force during drying can be achieved, and the purpose of atmospheric pressure drying can be achieved without solvent exchange. The process is simple, the cost is low, the equipment requirements are low, and it is easy to industrially mass produce. The prepared bagasse cellulose aerogel also has good mechanical strength and thermal insulation properties.
[0028] The bagasse cellulose aerogel prepared by the present invention is tested to have a volume density of ≤0.055 g / cm 3 ; Porosity ≥ 95%; Thermal conductivity ≤ 0.06W·m -1 ·K -1 ; Compressive strength ≥115kPa (at 50% strain).
[0029] Therefore, the present invention has the characteristics of simple process, low cost, short cycle, low equipment requirements, easy industrial production, high added value utilization of bagasse and preparation of bagasse cellulose aerogel of any size by normal pressure drying method; the prepared bagasse cellulose aerogel has low density, good hydrophobicity and excellent flame retardant performance, especially meets the requirements of high porosity and high strength, and is widely used in the fields of heat insulation, energy storage, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a real photo of a bagasse cellulose aerogel prepared by the present invention;
[0031] Figure 2 for Figure 1 FT-IR spectra of cellulose and bagasse cellulose aerogel are shown. DETAILED DESCRIPTION
[0032] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments, but is not intended to limit the scope of protection thereof.
[0033] A bagasse cellulose aerogel and a preparation method thereof. The preparation method described in this specific embodiment is:
[0034] Step 1, drying the cleaned bagasse in an oven at 80-85° C. for 22-24 hours to obtain dried bagasse; then crushing the dried bagasse, washing it with deionized water for 3-5 times, and then drying it at 80-90° C. for 22-24 hours to obtain pretreated bagasse.
[0035] Step 2: adding chitosan powder to acetic acid solution at a concentration of 1.9-2.1 wt%, stirring at a speed of 300-600 rpm for 2-3 hours to obtain a chitosan solution.
[0036] Step 3: placing the pretreated bagasse in a sodium hydroxide solution at a mass ratio of 1:30 to 50, stirring the pretreated bagasse at a speed of 300 to 600 rpm for 0.8 to 1.2 h in a water bath at 80 to 85° C., and then washing with deionized water until neutral to obtain product A.
[0037] Step 4: placing the product A in a sodium chlorite solution at a mass ratio of 1:30-50 to the pretreated bagasse and the sodium chlorite solution, adjusting the pH to 4.5-5 with acetic acid; then moving the product A to a water bath at 80-85° C. and stirring at a speed of 300-600 rpm for 0.8-1.2 h, then washing the product A with deionized water until neutral, and drying the product A at 80-85° C. for 4-6 h to obtain cellulose.
[0038] Step 5: preparing a cellulose suspension by stirring the mixture at a speed of 300 to 600 rpm for 12 to 24 hours at a mass ratio of cellulose to deionized water of 1:95 to 97.
[0039] Step 6: Add the chitosan solution into the cellulose suspension, stir evenly, and prepare suspension B; the chitosan solution is 20-60 wt % of the cellulose suspension.
[0040] Step 7, according to the mass ratio of suspension B to glutaraldehyde aqueous solution of 1: 0.01-0.055, the suspension B is added to the glutaraldehyde aqueous solution, stirred at a speed of 300-600 rpm for 10-30 seconds, poured into a mold, and after gelling, placed at -20--18°C for 45-48 hours, taken out, and allowed to stand at room temperature for 12-24 hours, and then dried in an oven at 80-85°C for 20-24 hours to obtain bagasse cellulose aerogel.
[0041] The concentration of the acetic acid solution is 0.9-1.1 wt %.
[0042] The concentration of the sodium hydroxide solution is 2-3 wt %.
[0043] The concentration of the sodium chlorite solution is 2-3 wt %.
[0044] The glutaraldehyde content in the glutaraldehyde aqueous solution is 23-27 wt %.
[0045] Example 1
[0046] A bagasse cellulose aerogel and a preparation method thereof. The preparation method described in this embodiment is:
[0047] Step 1, drying the cleaned bagasse in an oven at 80° C. for 24 hours to obtain dried bagasse; then crushing the dried bagasse, washing it with deionized water for 3 times, and then drying it at 80° C. for 22 hours to obtain pretreated bagasse.
[0048] Step 2: Add chitosan powder to acetic acid solution at a concentration of 1.9 wt %, and stir at 300 rpm for 2 h to obtain a chitosan solution.
[0049] Step 3: placing the pretreated bagasse in a sodium hydroxide solution at a mass ratio of 1:30, stirring at 300 rpm for 0.8 h in a water bath at 80° C., and then washing with deionized water until neutral to obtain product A.
[0050] Step 4: placing the product A in a sodium chlorite solution at a mass ratio of 1:30 between the pretreated bagasse and the sodium chlorite solution, adjusting the pH to 4.5 with acetic acid; then moving the product A to a water bath at 83° C. and stirring at 300 rpm for 0.8 h, then washing the product A with deionized water until neutral, and drying the product A at 83° C. for 4 h to obtain cellulose.
[0051] Step 5: The cellulose suspension is prepared by stirring at a speed of 300 rpm for 12 hours at a mass ratio of cellulose to deionized water of 1:95.
[0052] Step 6: Add the chitosan solution into the cellulose suspension, stir evenly, and prepare suspension B; the chitosan solution is 40 wt % of the cellulose suspension.
[0053] Step 7: Add the suspension B to the glutaraldehyde aqueous solution at a mass ratio of 1:0.01, stir at 300 rpm for 10 seconds, pour into a mold, place the gel at -20°C for 45 hours, take it out, let it stand at room temperature for 12 hours, and then dry it in an oven at 83°C for 20 hours to obtain bagasse cellulose aerogel.
[0054] The concentration of the acetic acid solution is 0.9 wt %.
[0055] The concentration of the sodium hydroxide solution is 3 wt %.
[0056] The concentration of the sodium chlorite solution is 3 wt %.
[0057] The glutaraldehyde content in the glutaraldehyde aqueous solution is 25 wt %.
[0058] The bagasse cellulose aerogel prepared in this example was tested and found to have a volume density of 0.055 g / cm 3; Porosity: 96.3%; Thermal conductivity: 0.06W·m -1 ·K -1 ; Compressive strength 213.4kPa (at 50% strain).
[0059] Example 2
[0060] A bagasse cellulose aerogel and a preparation method thereof. The specific steps of the preparation method described in this embodiment are:
[0061] Step 1, drying the cleaned bagasse in an oven at 85°C for 22 hours to obtain dried bagasse; then crushing the dried bagasse, washing it with deionized water for 4 times, and then drying it at 83°C for 23 hours to obtain pretreated bagasse.
[0062] Step 2: Add chitosan powder to acetic acid solution at a concentration of 2 wt %, and stir at 400 rpm for 2.5 h to obtain a chitosan solution.
[0063] Step 3: placing the pretreated bagasse in a sodium hydroxide solution at a mass ratio of 1:50, stirring at 400 rpm for 1.0 h in a water bath at 83° C., and then washing with deionized water until neutral to obtain product A.
[0064] Step 4: placing the product A in a sodium chlorite solution at a mass ratio of 1:50 between the pretreated bagasse and the sodium chlorite solution, adjusting the pH to 4.7 with acetic acid; then moving the product A to a water bath at 85° C. and stirring at 400 rpm for 0.9 h, then washing the product with deionized water until neutral, and drying the product at 84° C. for 5 h to obtain cellulose.
[0065] Step 5: The cellulose suspension is prepared by stirring at a speed of 400 rpm for 16 hours at a mass ratio of cellulose to deionized water of 1:97.
[0066] Step 6: Add the chitosan solution into the cellulose suspension, stir evenly, and prepare suspension B; the chitosan solution is 20 wt % of the cellulose suspension.
[0067] Step 7: Add the suspension B to the glutaraldehyde aqueous solution at a mass ratio of 1:0.03, stir at 400 rpm for 20 seconds, pour into a mold, place the gel at -19°C for 46 hours, take it out, let it stand at room temperature for 14 hours, and then dry it in an oven at 85°C for 21 hours to obtain bagasse cellulose aerogel.
[0068] The concentration of the acetic acid solution is 1.0 wt %.
[0069] The concentration of the sodium hydroxide solution is 2 wt %.
[0070] The concentration of the sodium chlorite solution is 2 wt %.
[0071] The glutaraldehyde content in the glutaraldehyde aqueous solution is 23 wt %.
[0072] The bagasse cellulose aerogel prepared in this example was tested and found to have a volume density of 0.046 g / cm 3 ; Porosity is 96.9%; Thermal conductivity is 0.052W·m -1 ·K -1 ; Compressive strength 117.8kPa (at 50% strain).
[0073] Example 3
[0074] A bagasse cellulose aerogel and a preparation method thereof. The preparation method described in this embodiment is:
[0075] Step 1, drying the cleaned bagasse in an oven at 82° C. for 23 hours to obtain dried bagasse; then crushing the dried bagasse, washing it with deionized water for 5 times, and then drying it at 85° C. for 24 hours to obtain pretreated bagasse.
[0076] Step 2: Add chitosan powder to acetic acid solution at a concentration of 2.1 wt%, and stir at 500 rpm for 2 h to obtain a chitosan solution.
[0077] Step 3: placing the pretreated bagasse in a sodium hydroxide solution at a mass ratio of 1:40, stirring at 500 rpm for 1.1 h in a water bath at 85° C., and then washing with deionized water until neutral to obtain product A.
[0078] Step 4: placing the product A in a sodium chlorite solution at a mass ratio of 1:40 between the pretreated bagasse and the sodium chlorite solution, adjusting the pH to 4.6 with acetic acid; then moving the solution to a water bath at 82° C. and stirring at 500 rpm for 1.0 h, then washing the solution with deionized water until neutral, and drying the solution at 82° C. for 6 h to obtain cellulose.
[0079] Step 5: The cellulose suspension is prepared by stirring at a speed of 500 rpm for 18 hours at a mass ratio of cellulose to deionized water of 1:96.
[0080] Step 6: Add the chitosan solution into the cellulose suspension, stir evenly, and prepare suspension B; the chitosan solution is 60 wt % of the cellulose suspension.
[0081] Step 7: according to the mass ratio of suspension B to glutaraldehyde aqueous solution of 1:0.04, the suspension B is added to the glutaraldehyde aqueous solution, stirred at a speed of 500 rpm for 30 seconds, poured into a mold, and the gel is placed at -18°C for 47 hours, taken out, and allowed to stand at room temperature for 20 hours, and then dried in an oven at 82°C for 22 hours to obtain bagasse cellulose aerogel.
[0082] The concentration of the acetic acid solution is 0.9 wt %.
[0083] The concentration of the sodium hydroxide solution is 3 wt %.
[0084] The concentration of the sodium chlorite solution is 3 wt %.
[0085] The glutaraldehyde content in the glutaraldehyde aqueous solution is 24 wt %.
[0086] The bagasse cellulose aerogel prepared in this example was tested and found to have a volume density of 0.042 g / cm 3 ; Porosity is 97.2%; Thermal conductivity is 0.054W·m -1 ·K -1 ; Compressive strength 217.8kPa (at 50% strain).
[0087] Example 4
[0088] A bagasse cellulose aerogel and a preparation method thereof. The preparation method described in this embodiment is:
[0089] Step 1, drying the washed bagasse in an oven at 84° C. for 24 hours to obtain dried bagasse; then crushing the dried bagasse, washing it with deionized water for 3 times, and then drying it at 88° C. for 22 hours to obtain pretreated bagasse.
[0090] Step 2: Add chitosan powder to acetic acid solution at a concentration of 2.1 wt%, and stir at 600 rpm for 3 h to obtain a chitosan solution.
[0091] Step 3: placing the pretreated bagasse in a sodium hydroxide solution at a mass ratio of 1:50, stirring at 600 rpm for 1.2 h in a water bath at 84° C., and then washing with deionized water until neutral to obtain product A.
[0092] Step 4: placing the product A in a sodium chlorite solution at a mass ratio of 1:50 between the pretreated bagasse and the sodium chlorite solution, adjusting the pH to 4.8 with acetic acid; then moving the product A to a water bath at 80° C. and stirring at 400 rpm for 1.1 h, then washing the product with deionized water until neutral, and drying the product at 80° C. for 4 h to obtain cellulose.
[0093] Step 5: The cellulose suspension is prepared by stirring at a speed of 400 rpm for 20 hours at a mass ratio of cellulose to deionized water of 1:97.
[0094] Step 6: Add the chitosan solution into the cellulose suspension, stir evenly, and prepare suspension B; the chitosan solution is 30 wt % of the cellulose suspension.
[0095] Step 7: Add the suspension B to the glutaraldehyde aqueous solution at a mass ratio of suspension B to glutaraldehyde aqueous solution of 1:0.055, stir at 400 rpm for 25 seconds, pour into a mold, place the gel at -18°C for 48 hours, take it out, let it stand at room temperature for 24 hours, and then dry it in an oven at 80°C for 23 hours to obtain bagasse cellulose aerogel.
[0096] The concentration of the acetic acid solution is 1.1 wt %.
[0097] The concentration of the sodium hydroxide solution is 2.5 wt %.
[0098] The concentration of the sodium chlorite solution is 2.5 wt %.
[0099] The glutaraldehyde content in the glutaraldehyde aqueous solution is 26 wt %.
[0100] The bagasse cellulose aerogel prepared in this example was tested and found to have a volume density of 0.047 g / cm 3 ; Porosity is 96.9%; Thermal conductivity is 0.055W·m -1 ·K -1 ; Compressive strength 218.1kPa (at 50% strain).
[0101] Example 5
[0102] A bagasse cellulose aerogel and a preparation method thereof. The preparation method described in this embodiment is:
[0103] Step 1, drying the washed bagasse in an oven at 83°C for 23 hours to obtain dried bagasse; then crushing the dried bagasse, washing it with deionized water for 5 times, and then drying it at 90°C for 24 hours to obtain pretreated bagasse.
[0104] Step 2: Add chitosan powder to acetic acid solution at a concentration of 2 wt %, and stir at 400 rpm for 2.5 h to obtain a chitosan solution.
[0105] Step 3: placing the pretreated bagasse in a sodium hydroxide solution at a mass ratio of 1:30, stirring at 500 rpm for 0.9 h in a water bath at 82° C., and then washing with deionized water until neutral to obtain product A.
[0106] Step 4: placing the product A in a sodium chlorite solution at a mass ratio of 1:30 between the pretreated bagasse and the sodium chlorite solution, adjusting the pH to 5 with acetic acid; then moving the product to a water bath at 84° C. and stirring at 600 rpm for 1.2 h, then washing the product with deionized water until neutral, and drying the product at 85° C. for 5 h to obtain cellulose.
[0107] Step 5: The cellulose suspension is prepared by stirring at a speed of 600 rpm for 24 hours at a mass ratio of cellulose to deionized water of 1:95.
[0108] Step 6: Add the chitosan solution into the cellulose suspension, stir evenly, and prepare suspension B; the chitosan solution is 50 wt % of the cellulose suspension.
[0109] Step 7: Add the suspension B to the glutaraldehyde aqueous solution at a mass ratio of 1:0.025, stir at 600 rpm for 30 seconds, pour into a mold, place the gel at -19°C for 48 hours, take it out, let it stand at room temperature for 18 hours, and then dry it in an oven at 84°C for 24 hours to obtain bagasse cellulose aerogel.
[0110] The concentration of the acetic acid solution is 1 wt %.
[0111] The concentration of the sodium hydroxide solution is 3 wt %.
[0112] The concentration of the sodium chlorite solution is 3 wt %.
[0113] The glutaraldehyde content in the glutaraldehyde aqueous solution is 27 wt %.
[0114] The bagasse cellulose aerogel prepared in this example was tested and found to have a volume density of 0.047 g / cm 3 ; Porosity is 97.2%; Thermal conductivity is 0.051W·m -1 ·K -1 ; Compressive strength 194.4kPa (at 50% strain).
[0115] Compared with the prior art, this specific implementation has the following positive effects and outstanding features:
[0116] 1. This specific implementation method uses bagasse as raw material and extracts bagasse cellulose through acid-base immersion etching. The raw material source is wide and concentrated, achieving high added value utilization of bagasse, low cost and green environmental protection; and the cellulose has low density and is degradable, and low-density, environmentally friendly and bagasse cellulose aerogel of any size can be prepared.
[0117] 2. This specific embodiment uses chitosan as a reinforcing agent to effectively enhance the connection strength between fibers and prevent fiber sliding, thereby improving the compressive elasticity and compressive strength of bagasse cellulose aerogel, and making the prepared bagasse cellulose aerogel have good hydrophobicity and flame retardancy.
[0118] 3. In this specific embodiment, glutaraldehyde is used as a cross-linking agent, and its aldehyde groups are cross-linked with the amino groups of chitosan and the hydroxyl groups on the surface of cellulose to build a strong connection, thereby preventing the collapse of the aerogel structure during normal pressure drying, ensuring the structural stability of the bagasse cellulose aerogel, and thus improving the compressive elasticity and mechanical properties.
[0119] 4. The present invention adopts the method of aging in a freezing environment to effectively prevent the evaporation of water in the gel, which not only has a higher porosity and a lower thermal conductivity, but also significantly shortens the preparation cycle of bagasse cellulose aerogel.
[0120] 5. In this specific embodiment, the cellulose aerogel is prepared by a normal pressure drying method. By adopting a more solid cross-linking method and increasing the pore size of the cellulose wet gel, the connection between the cellulose networks can be strengthened and the capillary force during drying can be reduced, so that the purpose of normal pressure drying can be achieved without solvent exchange. The process is simple, the cost is low, the equipment requirements are low, and it is easy to mass-produce industrially. The prepared aerogel also has good mechanical strength and thermal insulation properties. The bagasse cellulose aerogel prepared in this specific embodiment is as follows: Figure 1 As shown, Figure 1 This is a physical photo of the magnesium-aluminum spinel aerogel prepared in Example 1; Figure 2 for Figure 1 FT-IR spectra of cellulose and bagasse cellulose aerogel shown. Figure 1 It can be seen intuitively that the prepared magnesium-aluminum spinel aerogel is placed on flowers without bending the petals, indicating that the prepared magnesium-aluminum spinel aerogel has a small mass and low density. Figure 2 for Figure 1 FT-IR spectra of cellulose and cellulose bagasse aerogel shown in Figure 2. Figure 2 It can be seen that the bagasse cellulose aerogel 1570cm -1There is an obvious difference peak at , which is caused by the carbon-nitrogen double bond, which is generated by the reaction of the aldehyde group in glutaraldehyde and the amino group in chitosan. The strength of the aerogel comes from the cross-linking reaction between the aldehyde group of glutaraldehyde and the hydroxyl group on the surface of cellulose and the amino group of chitosan. Therefore, the bagasse cellulose aerogel prepared in this specific embodiment has low density, large porosity and high strength, which overcomes the problem of low strength of cellulose aerogel, has good hydrophobicity, excellent flame retardancy and excellent thermal insulation performance, and is widely used in insulation, energy storage and other fields.
[0121] The bagasse cellulose aerogel prepared in this specific embodiment is tested: the volume density is ≤0.055g / cm 3 ; Porosity
[0122] ≥95%; Thermal conductivity ≤0.06W·m -1 ·K -1 ; Compressive strength ≥115kPa (at 50% strain).
[0123] Therefore, the present specific implementation manner has the characteristics of simple process, low cost, short cycle, low equipment requirements, easy industrial production, high added value utilization of bagasse, and ability to prepare bagasse cellulose aerogel of any size by normal pressure drying method; the prepared bagasse cellulose aerogel has low density, good hydrophobicity and excellent flame retardant properties, especially meets the requirements of high porosity and high strength, and is widely used in the fields of heat insulation, energy storage, etc.
Claims
1. A method for preparing bagasse cellulose aerogel, characterized in that The steps of the preparation method are: Step 1, drying the cleaned bagasse in an oven at 80-85° C. for 22-24 hours to obtain dried bagasse; then crushing the dried bagasse, washing it with deionized water for 3-5 times, and then drying it at 80-90° C. for 22-24 hours to obtain pretreated bagasse; Step 2, adding chitosan powder to an acetic acid solution at a concentration of 1.9-2.1 wt%, stirring at a speed of 300-600 rpm for 2-3 hours to obtain a chitosan solution; Step 3, placing the pretreated bagasse in a sodium hydroxide solution at a mass ratio of 1:30-50, stirring at a speed of 300-600 rpm for 0.8-1.2 h in a water bath at 80-85° C., and then washing with deionized water until neutral to obtain product A; Step 4, according to the mass ratio of the pretreated bagasse to the sodium chlorite solution of 1:30-50, placing the product A in the sodium chlorite solution, adjusting the pH to 4.5-5 with acetic acid; then moving to a water bath at 80-85° C. and stirring at a speed of 300-600 rpm for 0.8-1.2 h, then washing with deionized water until neutral, and drying at 80-85° C. for 4-6 h to obtain cellulose; Step 5, according to the mass ratio of cellulose to deionized water being 1:95-97, stirring at a speed of 300-600 rpm for 12-24 hours to prepare a cellulose suspension; Step 6, adding the chitosan solution to the cellulose suspension, stirring evenly, to obtain suspension B; the chitosan solution is 20-60wt% of the cellulose suspension; Step 7, according to the mass ratio of suspension B to glutaraldehyde aqueous solution of 1: 0.01-0.055, the suspension B is added to the glutaraldehyde aqueous solution, stirred at a speed of 300-600 rpm for 10-30 s, poured into a mold, and after gelation, placed at -20--18°C for 45-48 h, taken out, and allowed to stand at room temperature for 12-24 h, and then dried in an oven at 80-85°C for 20-24 h to obtain bagasse cellulose aerogel.
2. The method for preparing bagasse cellulose aerogel according to claim 1, characterized in that The concentration of the acetic acid solution is 0.9-1.1 wt %.
3. The method for preparing bagasse cellulose aerogel according to claim 1, characterized in that The concentration of the sodium hydroxide solution is 2-3 wt %.
4. The method for preparing bagasse cellulose aerogel according to claim 1, characterized in that The concentration of the sodium chlorite solution is 2-3 wt %.
5. The method for preparing bagasse cellulose aerogel according to claim 1, characterized in that The glutaraldehyde content in the glutaraldehyde aqueous solution is 23-27wt%.
6. A bagasse cellulose aerogel, characterized in that The bagasse cellulose aerogel is a bagasse cellulose aerogel prepared by the method for preparing a bagasse cellulose aerogel according to any one of claims 1 to 5.