Antimony-magnesium-calcium composite treated cutting tool steel and preparation method thereof
By adding Ca, Mg, Sb to the cutting tool steel, the eutectic compound content of manganese antimony, manganese sulfide and antimony pentoxide, the problems of uneven distribution of inclusions and low fatigue performance in cutting tool steel are solved, and the more Good cutting performance and fatigue performance.
Patent Information
- Application Number
- CN202310307265.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-03-27
AI Technical Summary
The existing cutting tool steel has high inclusion content and uneven distribution, resulting in reduced cutting performance, lubricating performance, plasticity and fatigue strength, and no relevant research has been found in antimony, magnesium, calcium composite treatment process.
By adding Ca, Mg, Sb to the steel, the eutectic compounds content of manganese antimony, manganese sulfide and antimony pentoxide are controlled to form a composite wrapping, reducing the problem of excessive melting point caused by magnesium and alleviating the sulfation caused by evaporation of magnesium and calcium. Uneven manganese treatment solves the problem of fatigue performance and cutting performance reduction caused by increased calcium sulfide.
Effectively prevent water outlet blockage, improve the uniformity of inclusion distribution, improve cutting performance and fatigue performance, and improve the transverse and longitudinal mechanical properties of steel.
Smart Images

Figure CN116426848B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel smelting, and in particular relates to a cutting tool steel treated with antimony-magnesium-calcium composite treatment and a preparation method thereof. Background Art
[0002] Characteristics of cutting tool steel: Adding certain alloy elements to steel significantly improves the cutting performance, fatigue resistance, corrosion resistance and lubrication of the steel, and finally obtains a type of steel with good fatigue performance and cutting performance. Good cutting performance can effectively reduce the loss of cutting tools, reduce cutting resistance, increase service life, improve processing efficiency, and reduce production costs. This type of steel is widely used in mechanical parts, aerospace precision parts, precision instrument parts, electrical parts, machine tool parts, automobile transmission shafts, etc.
[0003] At present, the existing cutting tool steel has high inclusion content and uneven distribution, which seriously reduces the transverse and longitudinal mechanical properties of the steel, and reduces the cutting performance, lubrication performance, plasticity and fatigue strength of the steel. Up to now, there has been no report on the relevant research on improving the high inclusion content and uneven distribution in cutting tool steel through antimony-magnesium-calcium composite treatment process, thereby improving the cutting performance, lubrication performance, plasticity and fatigue performance. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a cutting tool steel treated with antimony-magnesium-calcium composite and a preparation method thereof.
[0005] The object of the present invention is achieved by the following methods:
[0006] The present invention provides a cutting tool steel treated with antimony-magnesium-calcium composite, which comprises, by mass percentage:
[0007] C: 0.60~0.68%, Si: 0.10~0.30%, Mn: 1.0~1.20%, P: 0.005~0.015%, S: 0.30~0.50%, Ca: 0.08~0.10%, Mg: 0.05~0.08%, Sb: 0.10~0.15%, Cu: 0.50~0.80%, Cr: 0.50~0.80%, and the rest are Fe and unavoidable impurity elements.
[0008] Based on the above technical solution, further, in the antimony-magnesium-calcium composite treated cutting tool steel, the mass ratio of manganese to sulfur is 2.0-3.5, the mass ratio of calcium to sulfur is 0.15-0.35, and the mass ratio of antimony to sulfur is 0.20-0.50.
[0009] The purpose of controlling the w[Ca] / w[S] mass ratio, the w[Mn] / w[S] mass ratio, and the w[Sb] / w[S] mass ratio in the present invention is to control the content of manganese antimonide, manganese sulfide, and antimony pentoxide, thereby controlling the content of eutectic compounds formed by manganese antimonide, manganese sulfide, and antimony pentoxide, reducing the problem of excessively high melting point caused by magnesium, and effectively preventing the occurrence of nozzle blockage; alleviating the problem of uneven treatment of manganese sulfide caused by the evaporation of magnesium and calcium, and at the same time, due to the composite coating formed by manganese antimonide, manganese sulfide and antimony pentoxide, solving the problem of reduced fatigue performance and cutting performance caused by increased calcium sulfide.
[0010] The present invention also provides a method for preparing the above-mentioned antimony-magnesium-calcium composite-treated cutting tool steel, which mainly includes the following steps: top and bottom combined blowing converter smelting → LF refining → continuous casting → heating → rolling → controlled cooling → coiling.
[0011] Based on the above technical solution, further, molten iron pretreatment is carried out before smelting in the top and bottom combined blowing converter. Since S is beneficial to the cutting performance of cutting tool steel, this type of steel does not need to be pre-desulfurized.
[0012] Based on the above technical solution, further, the raw materials for converter smelting are 12-15% scrap steel and 85-88% molten iron.
[0013] Based on the above technical scheme, further, the combined blowing converter smelting process: top blowing oxygen smelting, bottom blowing N2; molten steel tapping temperature 1680 ~ 1700 ℃, tapping end point C is controlled at 0.55% ~ 0.60%, P ≤ 0.005%, and slag is strictly prohibited.
[0014] Based on the above technical scheme, further, deoxidation alloying is carried out during the steel tapping process: 12-18 kg / t of lime is added when 1 / 5-1 / 3 of the steel is tapped, the bottom blowing gas is switched to Ar gas, the amount of alloy added per ton of steel: 3.0-5.0 kg / t of ferromanganese, 3.55-5.0 kg / t of ferroaluminum, and ferrochrome, ferroantimony and copper alloy are added during the steel tapping process.
[0015] Based on the above technical scheme, further, the LF refining process: under the premise of ensuring good slag fluidity, control the slag basicity R = 3.5 ~ 5.0, perform alloy fine-tuning on the molten steel, and ensure that the molten steel composition meets the target requirements; LF refining time 40min ~ 60min, full analysis temperature 1600℃ ~ 1620℃, auxiliary material addition amount per ton of steel: active lime 9 ~ 12Kg / t, carbide slag 0.20 ~ 0.3Kg / t steel, carbonized rice husk 0.60 ~ 0.80Kg / t, and the molten steel is tested from time to time, 0.15~0.30Kg / t of medium carbon ferromanganese is added to fine-tune the alloy, 1.10m~2.40m / t of sulfur wire is added, and at the same time, the Cr, Sb and Cu contents in the steel are guaranteed to be within the internal control range. After the refining is completed, the soft blowing time is ≥12min, 2.2~2.8m / t of silicon-calcium wire is fed, 1.1~2.4m / t of magnesium cored wire is added to make the Ca: 0.08~0.10% and Mg: 0.05~0.08% in the steel.
[0016] Based on the above technical scheme, further, the continuous casting process: the crystallizer electromagnetic stirring current is 250A, the frequency is 6Hz, forward and reverse rotation, the speed is 5 rpm, the platform temperature is 1625±10℃, the middle package temperature is 1525℃~1555℃, the superheat is maintained at 20℃~30℃, the pulling speed is 1.0m / min~1.2m / min; increase the cooling water volume to reduce sulfur segregation, the secondary cooling water volume is 0.4~0.5t water / t steel, the whole process is protected casting, and the crystallizer protective slag uses high carbon steel special protective slag; an electromagnetic stirrer is used for stirring at the end of solidification, and the ingot is flame cut.
[0017] Based on the above technical scheme, further, the heating process: using a step-by-step heating furnace for heating, the preheating section temperature is 930±20℃, the preheating time is 30~40min, the first heating section temperature is 1140±20℃, the heating time is 30~40min, the second heating section temperature is 1200±20℃, the heating time is 35~50min, the equalizing section temperature is 1200±20℃, the equalizing time is 40~50min, and the total heating time is ≤3.0h.
[0018] Based on the above technical solution, further, the rolling process: the starting rolling entrance temperature is 1130-1150°C; the final rolling temperature is 850-910°C.
[0019] Based on the above technical solution, the cooling process is further controlled: laminar cooling adopts rear-stage cooling, and the laminar cooling water is turned on from back to front in sequence to make the coiling temperature ≥600°C, and air cooling is performed after coiling to obtain a uniform and fine structure.
[0020] The beneficial effects of the present invention compared with the prior art are as follows:
[0021] 1. The present invention controls the amount of eutectic compounds formed by manganese antimonide, manganese sulfide and antimony pentoxide by adding Ca, Mg and Sb to steel, thereby reducing the problem of too high melting point caused by adding magnesium to steel and effectively preventing the occurrence of nozzle blockage;
[0022] 2. The present invention alleviates the problem of uneven treatment of manganese sulfide caused by evaporation of magnesium and calcium;
[0023] 3. The present invention solves the problem of reduced fatigue performance and cutting performance caused by increased calcium sulfide by using a composite package formed by manganese antimonide, manganese sulfide and antimony pentoxide. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention, the drawings related to the embodiments are briefly introduced below.
[0025] Figure 1 This is the inclusion distribution diagram of the antimony-magnesium-calcium composite-reinforced cutting tool steel obtained in Example 1;
[0026] Figure 2 This is a scanning electron microscope image of inclusions in the antimony-magnesium-calcium composite-reinforced cutting tool steel obtained in Example 2;
[0027] Figure 3 This is a scanning electron microscope image of the steel plate obtained in Example 1;
[0028] Figure 4 is the curve of the aspect ratio of manganese sulfide changing with the calcium-sulfur ratio;
[0029] Figure 5 The scanning electron microscope image of the inclusions in the steel obtained in Comparative Example 2;
[0030] Figure 6 This is the inclusion distribution diagram of the cutting tool steel of comparative example 3. DETAILED DESCRIPTION
[0031] The present invention is described in detail below with reference to the embodiments, but the embodiments of the present invention are not limited thereto. Obviously, the embodiments described below are only partial embodiments of the present invention. For those skilled in the art, other similar embodiments obtained without creative labor all fall within the protection scope of the present invention.
[0032] Embodiment 1:
[0033] A cutting tool steel treated with antimony-magnesium-calcium composite treatment, comprising, by mass percentage, 0.61% C, 0.12% Si, 1.05% Mn, 0.005% P, 0.31% S, 0.081% Ca, 0.052% Mg, 0.11% Sb, 0.54% Cu, 0.55% Cr, and the remainder being Fe and unavoidable impurity elements, wherein w[Mn] / w[S]=3.38, w[Ca] / w[S]=0.26, and w[Sb] / w[S]=0.35.
[0034] The production process of the cutting tool steel treated with antimony-magnesium-calcium composite treatment in the embodiment is: top and bottom combined blowing converter smelting → LF refining → continuous casting cc → heating → 2300mm hot rolling → controlled cooling → coiling → delivery;
[0035] The preparation method of the cutting tool steel treated with antimony-magnesium-calcium composite is as follows:
[0036] 1. Combined blowing converter (BOF) smelting: This steel grade does not require pre-desulfurization treatment, top blowing oxygen smelting, bottom blowing N2; molten steel tapping temperature 1682℃, tapping end point C: 0.56%, P: 0.003%, slag is strictly prohibited;
[0037] 2. Deoxidation and alloying: The steel outlet should be rounded, lime (15 kg / t steel) should be added when 1 / 5 of the steel is tapped, and the bottom blowing gas should be switched to Ar gas; the amount of alloy added per ton of steel: ferromanganese (3.12 kg / t steel), ferroaluminum (3.6 kg / t steel), and all the additions should be completed when 4 / 5 of the steel is tapped. In addition, ferrochrome, ferroantimony and copper alloy should be added during the tapping process.
[0038] 3. LF ladle furnace refining: Under the premise of ensuring good slag fluidity and maintaining a reducing atmosphere, feed the sulfur wire to adjust the sulfur content, then add ferrotellurium, blow argon at the bottom, and fine-tune the alloy of the molten steel to ensure that the composition of the molten steel meets the target requirements; LF refining time is 45 minutes, and the full analysis temperature is 1602℃. The amount of auxiliary materials added per ton of steel: 9.5Kg / t of active lime, 0.25Kg / t of calcium carbide slag, 0.65Kg / t of carbonized rice husk, and the molten steel is tested from time to time, 0.15Kg / t of medium carbon ferromanganese is added to fine-tune the alloy, and 1.17m / t of sulfur wire is added. At the same time, the Cr, Sb and Cu contents in the steel are guaranteed to be within the internal control range. At the end of refining, the soft blowing time is 12 minutes, 2.25m / t of silicon calcium wire is fed, and 1.11m / t of magnesium cored wire is added to make Ca: 0.081%, Mg: 0.052%,
[0039] 4. Continuous casting: 7 #Continuous casting machine casting, crystallizer electromagnetic stirring current 250A, frequency 6Hz, forward and reverse, speed 5 rpm. Platform temperature 1628℃, tundish temperature 1525℃~1545℃, superheat maintained at 20℃, 22℃, 23℃, casting speed 1.0m / min. Increase cooling water volume, reduce sulfur segregation, secondary cooling water volume 0.42t water / t steel, full protection casting, crystallizer protective slag uses high carbon steel special protective slag; electromagnetic stirrer is used for stirring at the end of solidification, and flame cutting is used for ingot.
[0040] 5. Heating process: Use walking beam heating furnace for heating, the preheating section temperature is 915℃, the preheating time is 32min, the first heating section temperature is 1125℃, the heating time is 30min, the second heating section temperature is 1185℃, the heating time is 40min, the soaking section temperature is 1184℃, and the soaking time is 40min.
[0041] 6. Rolling process: rolling inlet temperature: 1132℃; final rolling temperature: 890℃; coiling temperature: 680℃, laminar cooling adopts rear cooling, water meter number: 2, turn on the laminar cooling water from back to front, and air cool after coiling to obtain uniform and fine structure;
[0042] In order to ensure the quality of continuous casting billets, effective measures such as controlling the superheat of molten steel, billet drawing speed, electromagnetic stirring of the continuous casting crystallizer and electromagnetic stirring at the end are taken to improve the surface quality of the continuous casting billets, solving the problems of high inclusion content, uneven distribution, uneven transverse and longitudinal properties of the steel plate, and poor plasticity and toughness of the steel plate.
[0043] Comparative Example 1:
[0044] This comparative example provides a cutting tool steel, whose constituent elements and element weight percentages are C: 0.28%, Si: 0.06%, Mn: 1.4%, S: 0.1%, P: 0.08%, Ca: 0.03%, and the rest are Fe and unavoidable impurity elements, among which w[Mn] / w[S]=14, w[Ca] / w[S]=0.3.
[0045] The preparation method is the same as that of Example 1.
[0046] Comparative experimental analysis:
[0047] Figure 1 This is a scanning electron microscope image of the inclusion distribution of the antimony-magnesium-calcium composite reinforced cutting tool steel of Example 1. Figure 1 It can be seen that the finely dispersed MgO and Sb2O5 serve as the core of heterogeneous nucleation of manganese sulfide. Figure 3 This is a scanning image of the cutting tool steel treated with antimony-magnesium-calcium composite obtained in Example 1.
[0048] Comparative Example 1 lacks magnesium, calcium, antimony and other elements compared to Example 1. From the morphology and distribution of the inclusions in the product, it can be seen that the finely dispersed MgO and Sb2O5 of the antimony-magnesium-calcium composite reinforced cutting tool steel in Example 1 serve as the core of heterogeneous nucleation of manganese sulfide, promote the precipitation of sulfide, and the inclusion distribution is more uniform, and the cutting performance is better. In addition, it is not necessary to require that the entire MgO and Sb2O5 inclusions are completely transformed, as long as the outer layer with sufficient thickness completes the transformation, the need to improve the fatigue performance of the steel can be met.
[0049] Embodiment 2:
[0050] A cutting tool steel treated with antimony-magnesium-calcium composite treatment, comprising, by mass percentage, 0.63% C, 0.15% Si, 1.10% Mn, 0.007% P, 0.39% S, 0.089% Ca, 0.063% Mg, 0.13% Sb, 0.61% Cu, 0.63% Cr, and the remainder being Fe and unavoidable impurity elements, wherein w[Mn] / w[S]=2.82, w[Ca] / w[S]=0.23, and w[Sb] / w[S]=0.33.
[0051] The production process of the embodiment of the present invention is: top and bottom blowing converter smelting (BOF) → LF refining → continuous casting cc → heating → hot rolling → controlled cooling → coiling → delivery;
[0052] The preparation method of the cutting tool steel treated with antimony-magnesium-calcium composite is as follows:
[0053] 1. Combined blowing converter (BOF) smelting: This steel grade does not require pre-desulfurization treatment, top blowing oxygen smelting, bottom blowing N2; molten steel tapping temperature 1691 ° C, tapping end point C: 0.58%, P: 0.004%, slag is strictly prohibited;
[0054] 2. Deoxidation and alloying: The steel outlet should be rounded, lime 13 kg / t steel is added when 1 / 4 of the steel is tapped, and the bottom blowing gas is switched to Ar gas. The amount of alloy added per ton of steel: ferromanganese 3.9 kg / t steel, ferroaluminum 4.1 kg / t steel, which are added when 3 / 4 of the steel is tapped. In addition, ferrochrome, ferroantimony and copper alloy are added during the tapping process.
[0055] 3. LF ladle furnace refining: Under the premise of ensuring good slag fluidity and maintaining a reducing atmosphere, feed the sulfur wire to adjust the sulfur content, then add ferrotellurium and blow argon from the bottom. Fine-tune the alloy of the molten steel to ensure that the composition of the molten steel meets the target requirements; LF refining time is 50 minutes, and the full analysis temperature is 1610°C. The amount of auxiliary materials added per ton of steel: 10Kg / t of active lime, 0.25Kg / t of carbide slag, 0.71Kg / t of carbonized rice husk, and constantly monitor the molten steel, add 1.21m / t of sulfur wire, and add 0.21Kg / t of medium carbon ferromanganese to fine-tune the alloy. At the same time, ensure that the Cr, Sb and Cu contents in the steel are within the internal control range. At the end of refining, the soft blowing time is 14min, 2.5m / t of silicon calcium wire is fed, and 1.44m / t of magnesium cored wire is added to make Ca: 0.092%, Mg: 0.061%,
[0056] 4. Continuous casting: 7 # Continuous casting machine casting, crystallizer electromagnetic stirring current 250A, frequency 6Hz, forward and reverse, speed 5 rpm. Platform temperature 1632℃, tundish temperature 1531℃~1554℃, superheat maintained at 22℃, 25℃, 20℃, casting speed 1.1m / min. Increase cooling water volume, reduce sulfur segregation, secondary cooling water volume 0.51t water / t steel, full protection casting, high carbon steel special protective slag; electromagnetic stirrer is used for stirring at the end of solidification, and flame cutting is used for ingot.
[0057] 5. Heating process: Use walking beam heating furnace for heating, the preheating section temperature is 925℃, the preheating time is 37min, the first heating section temperature is 1131℃, the heating time is 32min, the second heating section temperature is 1190℃, the heating time is 38min, the soaking section temperature is 1195℃, and the soaking time is 40min.
[0058] 6. Rolling process: rolling inlet temperature: 1142℃; final rolling temperature: 900℃; coiling temperature: 690℃, laminar cooling adopts rear cooling, from back to front, open the layer cooling water, and air cool after coiling to obtain uniform and fine structure;
[0059] In order to ensure the quality of continuous casting billets, effective measures such as controlling the superheat of molten steel, billet drawing speed, electromagnetic stirring of continuous casting crystallizer and electromagnetic stirring at the end are taken to improve the surface quality of continuous casting billets and reduce the problems of high inclusion content, uneven distribution, uneven transverse and longitudinal properties of steel plates, and poor plasticity and toughness of steel plates.
[0060] Comparative Example 2:
[0061] The comparative example provides a cutting tool steel, the composition elements and element weight percentage of which are C: 0.32%, Si: 0.10%, Mn: 1.46%, S: 0.14%, P: 0.085%, Ca: 0.04%, and the rest are Fe and inevitable impurity elements. Among them, w[Mn] / w[S]=10.4, w[Ca] / w[S]=0.28.
[0062] The preparation method is the same as that in Example 2.
[0063] Comparative experimental analysis:
[0064] Figure 2 This is a scanning electron microscope image of the inclusions in the steel obtained in Example 2. Figure 2 It can be seen that finely dispersed magnesium oxide and antimony pentoxide serve as the core of the heterogeneous nucleation of manganese sulfide.
[0065] Comparative Example 2 lacks elements such as magnesium, calcium, and antimony compared to Example 2. From the morphology and distribution of inclusions in the product, it can be seen that the finely dispersed magnesium oxide and antimony pentoxide in Example 2 serve as the core of heterogeneous nucleation of manganese sulfide, promote the precipitation of sulfide, and the inclusion distribution is more uniform, and the cutting performance is better.
[0066] Comparative Example 2 greatly increases the content of calcium element compared to Example 2, resulting in the formation of calcium sulfide in the product of Comparative Example 2, which makes it easy for the nozzle to form nodules and also reduces the cutting performance. The degree of calcium treatment should not be too low. Insufficient calcium treatment causes inclusions to not become liquid phase, affecting the effect of manganese sulfide treatment, and further affecting the reduction of cutting performance. Figure 4 This is the curve of the length-to-width ratio of manganese sulfide changing with the calcium-sulfur ratio. When the calcium-sulfur ratio reaches a certain level, increasing the calcium treatment will not have a particularly significant effect on the morphology of manganese sulfide. On the contrary, an excessively large calcium-sulfur ratio will increase the formation of melting point inclusions such as calcium sulfide, which can easily clog the water nozzle and is not conducive to improving the cutting performance.
[0067] Figure 5 This is a scanning electron microscope image of the inclusions in the steel obtained in Comparative Example 2. Figure 5 It can be seen that excessive calcium treatment causes the formation of calcium sulfide inclusions.
[0068] Example 3: A cutting tool steel treated with an antimony-magnesium-calcium composite, calculated by mass percentage, includes: C: 0.68%, Si: 0.20%, Mn: 1.19%, P: 0.009%, S: 0.48%, Ca: 0.089%, Mg: 0.063%, Sb: 0.15%, Cu: 0.78%, Cr: 0.79%, and the rest are Fe and unavoidable impurity elements, among which w[Mn] / w[S]=2.48, w[Ca] / w[S]=0.18, w[Sb] / w[S]=0.31.
[0069] The production process of the embodiment of the present invention is: top and bottom blowing converter smelting (BOF) → LF refining → continuous casting cc → heating → hot rolling → controlled cooling → coiling → delivery;
[0070] The preparation method of the cutting tool steel treated with antimony-magnesium-calcium composite is as follows:
[0071] 1. Combined blowing converter (BOF) smelting: This steel grade does not require pre-desulfurization treatment, and is smelted by top blowing oxygen and bottom blowing N2; the molten steel tapping temperature is 1698℃, the tapping end point C: 0.60%, P: 0.006%, and slag is strictly prohibited;
[0072] 2. Deoxidation and alloying: The steel outlet should be round. When 1 / 3 of the steel is tapped, add lime (18 kg / t steel). The bottom blowing gas is switched to Ar gas. The amount of alloy added per ton of steel: 4.8 kg / t steel of ferromanganese and 4.9 kg / t steel of ferroaluminum. All the addition is completed when 2 / 3 of the steel is tapped. In addition, ferrochrome, ferroantimony and copper alloy are added during the tapping process.
[0073] 3. LF ladle furnace refining: Under the premise of ensuring good slag fluidity and maintaining a reducing atmosphere, feed the sulfur wire, then add antimony iron, and blow argon at the bottom. Fine-tune the alloy of the molten steel to make the composition of the molten steel meet the target requirements; LF refining time is 49 minutes, and the full analysis temperature is 1620℃. The amount of auxiliary materials added per ton of steel: 12Kg / t steel of active lime, 0.28Kg / t steel of calcium carbide slag, 0.78Kg / t steel of carbonized rice husk, and the molten steel is tested from time to time, 1.32m / t steel of sulfur wire is added, and 0.25Kg / t of medium carbon ferromanganese is added to fine-tune the alloy. At the same time, ensure that the Cr, Sb and Cu contents in the steel are within the internal control range. At the end of refining, the soft blowing time is 15min, 2.78m / t steel of silicon calcium wire is fed, and 1.84m / t steel of magnesium cored wire is added to make Ca: 0.10%, Mg: 0.078%,
[0074] 5. Continuous casting: 7 # Continuous casting machine casting, crystallizer electromagnetic stirring current 250A, frequency 6Hz, forward and reverse, speed 5 rpm. Platform temperature 1632℃, tundish temperature 1531℃~1554℃, superheat maintained at 22℃, 25℃, 20℃, casting speed 1.1m / min. Increase cooling water volume, reduce sulfur segregation, secondary cooling water volume 0.51t water / t steel, full protection casting, high carbon steel special protective slag; electromagnetic stirrer is used for stirring at the end of solidification, and flame cutting is used for ingot.
[0075] 6. Heating process: Use walking beam heating furnace for heating, the preheating section temperature is 931℃, the preheating time is 39min, the first heating section temperature is 1135℃, the heating time is 35min, the second heating section temperature is 1194℃, the heating time is 41min, the soaking section temperature is 1198℃, and the soaking time is 40min.
[0076] 7. Rolling process: rolling inlet temperature: 1145℃; final rolling temperature: 895℃; coiling temperature: 700℃, layer cooling adopts rear cooling, from back to front, open the layer cooling water, air cooling after coiling, so that the structure is uniform and fine;
[0077] In order to ensure the quality of continuous casting billets, measures such as controlling the superheat of molten steel, billet drawing speed, electromagnetic stirring of the continuous casting crystallizer and electromagnetic stirring at the end are taken to improve the surface quality of the continuous casting billets, solving the problems of high inclusion content, uneven distribution, uneven transverse and longitudinal properties of the steel plate, and poor plasticity and toughness of the steel plate.
[0078] Comparative Example 3:
[0079] The comparative example provides a cutting tool steel, the composition elements and weight percentage of which are C: 0.35%, Si: 0.15%, Mn: 1.52%, S: 0.22%, P: 0.012%, Ca: 0.045%, and the rest are Fe and inevitable impurity elements. Among them, w[Mn] / w[S]=6.91, w[Ca] / w[S]=0.20.
[0080] The preparation method is the same as that in Example 3.
[0081] Comparative experimental analysis:
[0082] Comparative Example 3 lacks magnesium, calcium, antimony and other elements compared to Example 3. The inclusion distribution diagram of the cutting tool steel of Comparative Example 3 is shown in FIG. Figure 6 The manganese sulfide has a large aspect ratio and a large deformation capacity, which reduces the cutting ability. Example 3 of the composite treatment of antimony, magnesium and calcium makes the spherical manganese antimonide and manganese sulfide evenly distributed, increases the hardness of manganese sulfide, reduces the deformation resistance during cutting, and has better cutting performance.
[0083] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A cutting tool steel treated with antimony-magnesium-calcium composite, It is characterized in that Calculated as mass percentage, including: C: 0.60-0.68%, Si: 0.10-0.30%, Mn: 1.0-1.20%, P: 0.005-0.015%, S: 0.30-0.50%, Ca: 0.08-0.10%, Mg: 0.05-0.08%, Sb: 0.10-0.15%, Cu: 0.50-0.80%, Cr: 0.50-0.80%, the rest are Fe and unavoidable impurity elements; In the antimony-magnesium-calcium composite treated cutting tool steel, the mass ratio of manganese to sulfur is 2.0-3.5, the mass ratio of calcium to sulfur is 0.15-0.35, and the mass ratio of antimony to sulfur is 0.20-0.50; The method for preparing the cutting tool steel treated with antimony-magnesium-calcium composite treatment mainly comprises the following steps: top and bottom combined blowing converter smelting → LF refining → continuous casting → heating → rolling → controlled cooling → coiling; Continuous casting process: platform temperature 1625±10℃, tundish temperature 1525℃~1555℃, superheat maintained at 20℃~30℃, casting speed 1.0m / min~1.2m / min; secondary cooling water volume 0.4~0.5t water / t steel, full protection casting; Heating process: adopt walking beam heating furnace for heating, preheating section temperature is 930±20℃, preheating time is 30~40min, first heating section temperature is 1140±20℃, heating time is 30~40min, second heating section temperature is 1200±20℃, heating time is 35~50min, soaking section temperature is 1200±20℃, soaking time is 40~50min, total heating time is ≤3.0h; Rolling process: the inlet temperature of the first rolling is 1130-1150℃; the final rolling temperature is 850-910℃; Controlled cooling process: Laminar cooling uses rear cooling to make the coiling temperature ≥ 600℃, and air cooling after coiling.
2. The cutting tool steel treated with antimony-magnesium-calcium composite according to claim 1, It is characterized in that Top and bottom combined blowing converter smelting process: top blowing oxygen smelting, bottom blowing N 2 ; The tapping temperature of molten steel is 1680~1700℃, the tapping end point C is controlled at 0.55%~0.60%, P≤0.005%, and slag is strictly prohibited.
3. The cutting tool steel treated with antimony-magnesium-calcium composite according to claim 1, It is characterized in that Deoxidation and alloying are carried out during the steel tapping process: 12-18 kg / t of lime is added when 1 / 5-1 / 3 of the steel is tapped, the bottom blowing gas is switched to Ar gas, the amount of alloy added per ton of steel: 3.0-5.0 kg / t of ferromanganese, 3.55-5.0 kg / t of ferroaluminum. During the steel tapping process, ferrochrome, ferroantimony and copper alloy are added.
4. The cutting tool steel treated with antimony-magnesium-calcium composite according to claim 1, It is characterized in that LF refining process: Under the premise of ensuring good slag fluidity, control the slag basicity R=3.5~5.0; LF refining time is 40min~60min, full analysis temperature is 1600℃~1620℃, after refining, soft blowing time is ≥12min, silicon calcium wire and magnesium cored wire are fed to make Ca: 0.08~0.10%, Mg: 0.05~0.08% in steel.