A controllable grafted styrene secondary modified super-hydrophobic cotton fabric and preparation method thereof
By carrying out controlled grafting of styrene secondary modification on cotton fabrics and using perfluoropolyether carboxylic acid to improve the hydrophobic properties, the problems of hydrophilicity and susceptibility to stains on cotton fabrics were solved, and superhydrophobic properties and excellent oil-water separation were achieved. efficiency.
Patent Information
- Application Number
- CN202310562703.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-05-18
AI Technical Summary
The hydrophilic nature of cotton fabrics, susceptibility to mildew, and flammability limit their application scope, and the properties of existing fabrics obtained by grafting need to be improved.
A method of secondary modification of superhydrophobic cotton fabric by controlled grafting of styrene is used. The bromine source reacts with the cotton fabric to introduce ATRP reactive groups, which then react with styrene to form a rough surface. Perfluoropolyether carboxylic acid is then used for secondary modification. Secondary modification to improve the hydrophobic properties of the fabric.
Significantly improved the oil-water separation efficiency and friction fastness of the fabric. The contact angle increased from 144.8 ± 3.6° to 155.2 ± 3.5°. After 10 oil-water separation cycle tests, the oil-water separation efficiency remained at 98.6% without changing the microstructure of the fiber. .
Smart Images

Figure CN116427172B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to fabric processing technology, and specifically relates to a controllable grafted styrene secondary modified super-hydrophobic cotton fabric and a preparation method thereof. Background Art
[0002] As we all know, cotton fabric is a hydrophilic fabric that is easily soaked by water. It is also susceptible to other liquid stains and has disadvantages such as easy to mold and flammable, which limits its application range. To overcome these shortcomings, researchers have functionally finished cotton fabrics to make them antibacterial, self-cleaning, anti-icing, and conductive. There are simple coating methods for hydrophobic finishing of cotton fabrics, such as electrospinning, spraying, sol-gel method and other physical methods, as well as chemical grafting reactions. By utilizing the reactivity of the hydroxyl groups on the surface of cotton fibers and accessing different types of functional monomers, super-hydrophobic fabrics can be achieved. However, the performance of fabrics obtained by existing grafting treatments needs to be improved. Summary of the invention
[0003] The invention discloses a controllable grafted styrene secondary modified super hydrophobic cotton fabric and a preparation method thereof, wherein the contact angle of the PS modified cotton fabric is increased from 144.8 ± 3.6° to 155.2 ± 3.5° by secondary hydrophobic modification with perfluoropolyether carboxylic acid, showing super hydrophobic performance. The finished fabric has excellent oil-water separation performance, and after 10 oil-water separation cycle tests, its oil-water separation efficiency remains at 98.6%.
[0004] The present invention adopts the following technical solution:
[0005] A method for preparing a controllable grafted styrene secondary modified super-hydrophobic cotton fabric comprises the following steps: reacting a bromine source with cotton fabric to obtain cotton-Br; then reacting styrene with cotton-Br to obtain cotton-PS; and then reacting cotton-PS with perfluoropolyether carboxylic acid to obtain a controllable grafted styrene secondary modified super-hydrophobic cotton fabric.
[0006] In the present invention, the bromine source is an organic bromine compound, such as 2-bromoisobutyryl bromide; the alkalized cotton fabric is obtained by treating the original cotton fabric with sodium hydroxide. Preferably, the mass ratio of the bromine source to the cotton fabric is (0.5-2.5):1, preferably (1.5-2.2):1.
[0007] In the present invention, the temperature of the reaction of the bromine source and the cotton fabric is 5-45°C, and the time is 5-30 hours. Preferably, the reaction is carried out at 5°C to room temperature for 1-5 hours, and then at room temperature to 45°C for 20-25 hours.
[0008] In the present invention, the reaction of the bromine source and the cotton fabric is carried out in the presence of an organic base and an organic catalyst, preferably, the organic base is triethylamine, and the organic catalyst is a pyridine compound, such as 4-dimethylaminopyridine. The amount of the organic catalyst is 1 to 8% of the mass of the cotton fabric, preferably 3 to 6%, such as 4 to 5%.
[0009] In the present invention, the reaction of styrene and cotton-Br is carried out in an organic solvent; preferably, when styrene reacts with cotton-Br, the concentration of styrene is 0.1-1 mol / L, preferably 0.5-1 mol / L, and more preferably 0.6-0.8 mol / L; preferably, when styrene reacts with cotton-Br, the bath ratio is 1:(50-150), preferably 1:(100-130).
[0010] In the present invention, the reaction of styrene and cotton-Br is carried out in the presence of an organic ligand and a copper salt; preferably, the organic ligand is PMDETA and the copper salt is cuprous bromide; preferably, the mass ratio of cotton-Br, the organic ligand and the copper salt is 1:(0.8-1.2):(1-1.5), preferably 1:(0.9-1.1):(1.2-1.3).
[0011] In the present invention, the reaction temperature of styrene and cotton-Br is 30 to 100° C., preferably 50 to 60° C.; the reaction time is 5 to 30 hours, preferably 8 to 24 hours, and more preferably 10 to 16 hours.
[0012] In the present invention, the reaction of cotton-PS and perfluoropolyether carboxylic acid is carried out under the catalysis of an organic base, and the preferred organic base is DBU; preferably, the mass ratio of cotton-PS, perfluoropolyether carboxylic acid, and DBU is 1: (1.5-3): (0.1-0.2), preferably 1: (1.8-2.5): (0.12-0.15).
[0013] In the present invention, the molecular weight of the perfluoropolyether carboxylic acid is 500 to 20,000, preferably 500 to 1,200, and more preferably 500 to 750.
[0014] In the present invention, the reaction temperature of cotton-PS and perfluoropolyether carboxylic acid is 80-100° C. and the reaction time is 10-15 hours.
[0015] The invention discloses application of the controllably grafted styrene secondary modified super-hydrophobic cotton fabric in preparation or as a hydrophobic material.
[0016] The invention discloses application of the controllably grafted styrene secondary modified super-hydrophobic cotton fabric in the preparation or as an oil-water separation material.
[0017] The present invention uses 2-bromoisobutyryl bromide to react on alkalized cotton fabric, so that ATRP reactive groups are introduced into the cotton fabric, DMF is used as a reaction solvent, styrene polymerization is initiated under a PMDETA / CuBr system, and a rough surface is constructed on the cotton fabric. Perfluoropolyether carboxylic acid is used for secondary modification to prepare super-hydrophobic cotton fabric. The effects of reaction solution bath ratio, monomer concentration and grafting time are studied by SEM and WCA test characterization. The results show that cotton fabrics with better rough morphology can be obtained when the reaction solution bath ratio is 1:120, the monomer concentration is 0.75 mol / L, and the reaction time is more than 8 h. With the increase of grafting time, the contact angle to water can increase to 144.8 ± 3.6°. The successful reaction is proved by EDS, FT-IR and AFM. AFM shows that a rough surface with a surface roughness Rq = 61.6 nm can be constructed by ATRP grafting styrene. The presence of the rough surface makes the cotton fabric change from hydrophilic to hydrophobic. The secondary modification of perfluoropolyether carboxylic acid increased the water contact angle from 144.8 ± 3.6° to 155.2 ± 3.5°. EDS, FT-IR and XPS proved the successful reaction. The prepared super hydrophobic fabric has excellent oil-water separation efficiency and friction fastness. After 10 oil-water separation cycle tests, its oil-water separation efficiency remains at 98.6%. XRD test proves that the grafting modification of cotton fabric basically occurs on the fiber surface, and does not damage or change the fiber's microstructure.
[0018] The present invention uses controllable grafting of styrene to construct a rough morphology on the fiber surface, and further uses perfluoropolyether carboxylic acid for secondary hydrophobic modification. The rough physical structure generated by controllable grafting on the fiber surface can wrap air when the fabric contacts water droplets, greatly reducing the direct contact area between the fiber and the water droplets, and combined with the low surface energy chemical elements provided by perfluoropolyether, a super hydrophobic function is provided. This is a beneficial effect of the scheme of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is the experimental process of grafting modification and secondary modification.
[0020] Figure 2 IR and EDS characterization of cotton-Br macroinitiator: (a) IR; (b) EDS.
[0021] Figure 3 SEM images of cotton-Br macromolecular initiator and water contact angle test: (a) raw cotton; (b) cotton-Br macromolecular initiator.
[0022] Figure 4 Effects of different reaction bath ratios on the morphology (concentration is 0.5 mol / L, reaction time is 8 h): (a, a1) 1:50; (b, b1) 1:120.
[0023] Figure 5 Effects of different monomer concentrations on fabric morphology and water contact angle (bath ratio of reaction solution is 1:120, reaction time is 12 h): (a, a1) 0.5 mol / L; (b, b1) 0.75 mol / L.
[0024] Figure 6 Effects of different grafting times on the surface morphology of cotton fabrics (reaction solution bath ratio of 1:120, concentration of 0.75 mol / L): (a) 8 h; (b) 12 h; (c) 16 h; (d) 24 h.
[0025] Figure 7 The effect of different grafting times on the hydrophobicity of cotton fabric surface.
[0026] Figure 8 SEM and AFM of cotton fabric after ATRP grafting: (a) SEM; (b, c) 3D images at different angles.
[0027] Fig. 9 Infrared characterization of cotton-PS-PFPE: (a) cotton; (b) cotton-Br; (c) cotton-PS; (d) cotton-PS-PFPE.
[0028] Fig.10 EDS test of cotton fabric modified with PFPE-COOH of different molecular weights: (a) molecular weight 750; (b) molecular weight 500.
[0029] Fig.11 XPS for modified cotton fabrics: (a) cotton-PS; (b) cotton-PS-PFPE.
[0030] Fig.12 Shows the TGA curves of cotton fabrics before and after secondary modification.
[0031] Fig.13 XRD test of cotton fabric before and after modification: (a) Cotton; (b) Cotton-Br; (c) Cotton-PS; (d) Cotton-PS-PFPE.
[0032] Fig.14 SEM and AFM of cotton fabric after secondary modification: (a) SEM; (b, c) 3D images at different angles.
[0033] Fig.15 Oil-water separation and self-cleaning properties of cotton fabric after treatment: (a) oil-water separation process diagram; (b) methylene blue; (c) chalk dust; (d) oil-water separation efficiency after 10 cycles.
[0034] Fig.16 This is the test result of the modified fabric of comparative example 2. DETAILED DESCRIPTION
[0035] The present invention utilizes 2-bromoisobutyryl bromide to access ATRP reaction active sites on the fiber surface, and through ATRP reaction, styrene is used as a monomer to graft modified fibers. The grafting reaction process is controlled to form a rough morphology in situ on the fiber surface. C-Br on the graft surface can condense with perfluoropolyether carboxylic acid, and DBU is introduced during the reaction to activate the perfluoropolyether carboxylic acid, thereby obtaining a super-hydrophobic cotton fabric. The obtained super-hydrophobic cotton fabric is tested for chemical composition, surface morphology, contact angle, surface roughness, self-cleaning and oil-water separation performance.
[0036] The experimental reagents and raw materials used in the present invention are all existing products, and the specific preparation operations and performance tests are conventional methods, as shown in Table 1.
[0037]
[0038] X-ray photoelectron spectroscopy (XPS) analysis was performed using a monochromatic AlKa source with an energy of 1486.6 eV, a voltage of 15 kV, and a beam current of 10 mA. The pressure was set to 4.0 × 10 -9 Pa.
[0039] Scanning electron microscope (SEM) test: The surface morphology of the coating prepared on the fabric was tested and observed by SEM. A sample of suitable size was attached to the sample stage using conductive adhesive and gold sprayed for 1.5 min. The fabric sample was gold sprayed 3 times. The sample was placed in a scanning electron microscope for observation, and after magnification to a suitable multiple, it was photographed. The size distribution of the microspheres was analyzed using Image J software. 100 microspheres were randomly selected from the SEM image for particle size measurement, and the analysis results were expressed as average particle size ± standard deviation.
[0040] Static contact angle (WCA) and rolling angle tests, the prepared fabric coating was subjected to contact angle tests. The fabric was cut into appropriate sizes and adhered to a glass slide with double-sided tape. A 5 μL water droplet was used as the test droplet. A high-speed camera was used to record the shape of the water droplet when it contacted the sample surface, and the data was recorded and the average value and error were calculated.
[0041] Energy dispersive X-ray spectroscopy (EDS) testing uses the energy dispersive X-ray spectrometer on the built-in scanning electron microscope of 8100 for testing and analysis. The sample preparation method is the same as the scanning electron microscope test.
[0042] Thermogravimetric (TGA) analysis The thermal properties of raw cotton and finished fabrics were analyzed using a thermogravimeter. The sample was cut into small pieces, about 5 mg was placed in a crucible, and then placed in the instrument for testing. The test atmosphere was nitrogen, the test temperature range was 30 ~ 600℃, and the heating rate was 10℃ / min.
[0043] For fabric XRD analysis, the samples were glued to a glass / aluminum sample stage and tested using an X-ray diffractometer with a test range of 5 - 60°, a scan rate of 10 ° / min, a light source of Cu-Kα rays, a tube voltage of 40 kV, and a current of 40 mA.
[0044] Atomic force microscopy (AFM) test: The three-dimensional structure of the surface structure of the prepared sample is observed using an atomic force microscope. The sample cut to a certain size is pasted on the sample stage using double-sided tape, and then observed using an atomic microscope and the roughness of the sample surface is calculated using software, with the scanning range set to 0.8 μm × 0.8 μm.
[0045] Oil-water separation, self-cleaning and anti-fouling tests of coated fabrics:
[0046] Oil-water separation experiment: Use n-heptane dyed with oil red and deionized water dyed with methylene blue as the oil and water agents in the test process respectively. Fix the coated cotton fabric in the middle of the upper and lower glass tubes of the oil-water separator as the filter membrane for oil-water separation. Take 10 mL of oil and 10 mL of water in a measuring cylinder, pour the oil and water into the glass tube, observe the effect of oil-water separation, and record the separation efficiency.
[0047] Self-cleaning test: Methylene blue powder is used as the test pollutant. During the test, the coated cotton fabric is fixed on a glass slide and placed at an angle. Then a syringe is used to slowly inject water droplets onto the coating surface to observe the cleaning phenomenon of the surface pollutants.
[0048] (3) Anti-fouling test: Immerse the fabric in an aqueous solution dyed with methylene blue for 1 min, then take it out and observe the stain on the fabric surface.
[0049] Fabric air permeability test The air permeability of cotton fabrics before and after coating was tested using a fully automatic air permeability meter. The test parameters are: test pressure: 160 Pa, test area: 20 cm 2 , caliber: 4Φ. Each sample was tested 5 times to get the average value.
[0050] The technical route of the present invention is as follows Figure 1 As shown. 2-Bromoisobutyryl bromide is connected to the ATRP reaction active site on the fiber surface, and styrene is used as a monomer to graft and modify the fiber to form a rough morphology through ATRP reaction; the terminal C-Br introduced by grafting is then reacted with perfluoropolyether carboxylic acid to prepare superhydrophobic cotton fabric.
[0051] Add 100 g of sodium hydroxide and 500 mL of deionized water into a 1000 mL beaker and stir until dissolved. Place the original cotton fabric in the sodium hydroxide solution for 1 h, take it out and wash it 5 times with deionized water. Place the alkalized cotton fabric in 5% glacial acetic acid for 30 min, then rinse it with deionized water several times and dry it at room temperature. The obtained cotton fabric is used in the following experiments. Embodiment 1
[0052] In a three-necked flask, add 1.0 g of cotton fabric and 50 g of ultra-dry tetrahydrofuran, add 1.23 mL of ultra-dry triethylamine, and 0.5 g of 4-dimethylaminopyridine, place the three-necked flask in an ice bath, cool to 10°C, evacuate, and under nitrogen protection, drop 1.11 mL of 2-bromoisobutyryl bromide, drop it in 5 minutes, keep it at 10°C for 2 h, and then transfer it to an oil bath pot at 35°C for 24 h. After the reaction, wash the cotton cloth in anhydrous ethanol three times, then place it in a vacuum oven at 45°C and dry it to obtain cotton-Br.
[0053] Taking the bath ratio of 1:120 and the styrene concentration of 0.75 mol / L as an example: 745 mg of cotton fabric (cotton-Br) was placed in a sealed three-necked flask equipped with a magnetic stirrer in advance, and 745 mg of cuprous bromide was added under a nitrogen atmosphere; then, ultra-dry DMF (8.94 mL) and styrene (697 mg) monomers that had been ultrasonically deoxygenated were added, and the vacuum-nitrogen flow was repeated three times. Under vacuum, 900 mg of PMDETA was added, and the temperature was raised to 50°C. The reaction was carried out for the set time. After the reaction was completed, the three-necked flask was placed in an ice bath for rapid cooling, and then the fabric was taken out and repeatedly washed with anhydrous methanol, anhydrous ethanol and deionized water for 3 times until the solution was clear; finally, the fabric was dried in a vacuum oven to obtain a modified cotton fabric (cotton-PS).
[0054] By changing the bath ratio of the reaction solution, styrene concentration and reaction time, different modified fabrics were obtained and their morphology and hydrophobicity were studied; the bath ratio was cotton mass: reaction solution volume.
[0055] Take the grafted perfluoropolyether carboxylic acid with a molecular weight of 500 as an example: 1.0 g of modified cotton fabric (cotton-PS) was added to a three-necked flask, and then 2.0 g of perfluoropolyether carboxylic acid, 30.0 g of benzene and 30.0 g of 1,3-bis(trifluoromethyl)benzene were added. The device was then sealed, evacuated, and protected with nitrogen. After the perfluoropolyether carboxylic acid was completely dissolved, 146 mg of DBU was added, and then the reaction was carried out at 90°C for 12 h. After the reaction, the fabric was repeatedly washed three times in anhydrous methanol and ethanol, and then dried in a vacuum oven to obtain a super-hydrophobic cotton fabric grafted with styrene for a second time (cotton-PS-PFPE).
[0056] Referring to the above method, the grafted molecular weight of perfluoropolyether carboxylic acid was changed to obtain different finished cotton fabrics and study their properties.
[0057] (1) IR and EDS characterization of cotton-Br
[0058] The cotton fabric treated with 2-bromoisobutyryl bromide was subjected to infrared testing and EDS spectrum analysis. Figure 2 As shown in the infrared image, 3350 cm -1 The peak at 2900 cm is the stretching vibration peak of the hydroxyl group on the cotton fiber. -1 is the stretching vibration of -CH-, 1651cm -1 is the hydroxyl peak of cotton fiber adsorbing water molecules. Compared with the original cotton fabric, cotton-Br at 1741 cm -1 The peak at is the stretching vibration peak of carbonyl C=O, which proves that 2-bromoisobutyryl bromide successfully reacts with the hydroxyl groups on the cotton fabric. In addition, the EDS results show that the surface elements of the treated cotton fabric are only C, O, and Br, and the weights (%) of the three elements are 64.05%, 34.73%, and 1.21%, respectively. The bromine content is relatively small. In summary, the cotton-Br macromolecular initiator was successfully prepared.
[0059] The synthesized cotton-Br macroinitiator was tested by SEM. Figure 3 As shown. The introduction of ATRP grafting sites on cotton fabric did not affect the morphology of cotton fabric. The contact angle test was 125.8 ± 2.7°. As we all know, raw cotton is a hydrophilic fiber. This phenomenon also indirectly indicates that the preparation of cotton-Br macromolecular initiator was successful.
[0060] The grafting morphology of different reaction bath ratios was studied when the styrene concentration was 0.5 mol / L and the reaction time was 8 h. Figure 4 As shown, (a, a1) is the morphology formed when the bath ratio is 1:50, and (b, b1) is the morphology when the bath ratio is 1:120. When the bath ratio of fabric to reaction solvent is 1:120, it is easier to form a filamentous morphology on the fabric. Unless otherwise specified, the bath ratio of the reaction solution in the following experiments is 1:120.
[0061] The other conditions were kept constant, the bath ratio of the reaction solution was 1:120, and the reaction time was 12 h. The hydrophobicity of cotton fabrics prepared with different styrene concentrations was studied. The SEM images and contact angles of the fabrics after the reaction were shown in Figure 2. Figure 5 As shown in the figure, it can be seen that when the concentration is 0.5 mol / L, the contact angle of the fabric to water after the reaction is 133.1 ± 1.9°; and when the concentration is 0.75 mol / L, the contact angle of the fabric to water after the reaction is 136.9 ± 2.1°, and the contact angle is slightly improved. Figure 5In (a), the fabric surface is a film, and no obvious rough morphology is found. Figure 5 In (b), the fabric surface has a filamentous structure.
[0062] Keeping other conditions unchanged, the bath ratio of the reaction solution was 1:120, and the concentration of styrene was 0.75 mol / L. The morphology and hydrophobicity of the fabrics prepared with different reaction times were studied. The results are as follows: Figure 6 shown. Figure 6 (ad) correspond to the SEM images at 8 h, 12 h, 16 h, and 24 h of reaction, respectively. As the reaction time increases, the number of filamentous structures on the fabric surface increases.
[0063] Figure 7 The contact angle of cotton fabric surface with different grafting time is shown in Figure 1. The contact angle of cotton-Br macromolecular initiator to water is 125.8 ± 2.7°. After 8 h of introducing styrene chain segments by ATRP method, WCA increases to 137.7 ± 1.6°. With the extension of reaction time, the contact angle increases. After 16 h and 24 h of reaction, the contact angle increases to about 144°.
[0064] The modified cotton fabric prepared at a reaction liquid bath ratio of 1:120, a monomer concentration of 0.75 mol / L, and an ATRP reaction time of 12 h was subjected to an atomic force microscope test to characterize the change in the surface roughness of the fabric. The scanning range in the test was 0.8 μm × 0.8 μm. The test results are shown in Figure 2. Figure 8 shown. Figure 8 (b) and (c) are 3D images at different angles. It can be seen from the figure that the surface of cotton fiber without polystyrene grafting is smooth, which is completely different from the roughness of the filamentous structure. Through testing, it can be seen that the roughness Rq of cotton fabric is 68.1 nm. This is because styrene polymerizes and cross-links under ATRP conditions to form a filamentous structure, which greatly increases the roughness of the fabric surface. Therefore, compared with cotton-Br macromolecular initiator, the contact angle of the fabric after grafting PS is improved.
[0065] Infrared tests were performed on cotton-PS and secondary modified cotton-PS-PFPE. The results are as follows: Fig. 9 As shown, at 3346cm -1 is the stretching vibration peak of the associated -OH; 3026 cm -1 To 2854 cm -1 The stretching vibration peak of unsaturated CH on the benzene ring; 1734 cm -1 is the stretching vibration of -C=O in the ester group; 1056 cm -1 To 1235 cm -1 It is the characteristic absorption peak of CF, which shows that perfluoropolyether is successfully introduced into the fabric surface.
[0066] Perfluoropolyether carboxylic acid with molecular weight of 500 and 750 was used to modify polystyrene grafted cotton fabrics, and EDS was used to characterize the fluorine content on the surface of the cotton fabrics after secondary modification, which can also indirectly verify the successful introduction of PFPE-COOH. Fig.10 As shown in the figure, the proportion of fluorine on the surface of cotton fabric (a) after secondary modification with PFPE-COOH with a molecular weight of 750 is 2.97%, which is higher than that of cotton fabric (b) after secondary modification with PFPE-COOH with a molecular weight of 500. Correspondingly, the contact angles of cotton fabrics to water after modification are also different, and the contact angles of cotton fabrics after secondary modification are 152.3 ± 1.7° and 155.2 ± 3.5°, respectively.
[0067] XPS tests were performed on cotton-Br grafted with styrene and cotton-PS-PFPE secondary modified with perfluoropolyether carboxylic acid with a molecular weight of 500. The test results are shown in Fig.11 There is an obvious F at 685.08 eV. 1s The characteristic peak of O 1s At 532.71 eV, C 1s At around 285.42 eV, the F 1s The content is 1.92%, Br 3d The proportion is 0.07%, C 1s The proportion is 71.34%, 1s The proportion is 26.67%. In cotton-PS without perfluoropolyether carboxylic acid modification, C 1s Elements are 76.34%, O 1s The element accounts for 21.43%, Br 3d The change in the content of these elements indicates that after the fabric is modified with perfluoropolyether carboxylic acid, fluorine-containing substances are deposited on the surface of the fabric. This result also indirectly indicates that perfluoropolyether carboxylic acid is successfully grafted onto cotton fabric.
[0068] TGA was used to characterize the thermal stability of cotton fabrics before and after modification. The obtained TGA curves are shown in Fig.12 As shown in the figure, the initial degradation temperatures of the two fabrics are 345℃ and 340℃, respectively, with almost no difference, but the final decomposition temperatures are different. The final decomposition temperatures of the original cotton fabric and the grafted modified cotton fabric are 392℃ and 445℃, corresponding to residual carbon rates of 5.77% and 11.66%. TGA test shows that the introduction of perfluoropolyether increases the final decomposition temperature due to the larger bond energy of CF bond, which indicates that due to the good thermal stability of perfluoropolyether, its introduction can improve the heat resistance of cotton fabric to a certain extent.
[0069] The X-ray diffraction curves of raw cotton fabric, cotton-Br, cotton-Ps and cotton-PS-PFPE are shown in Fig.13 As shown in the figure, the XRD curves of cotton-Br, cotton-PS and cotton-PS-PFPE are basically consistent with those of cotton fabrics, with almost no change, which shows that the grafting modification of cotton fabrics basically occurs on the fiber surface and does not cause loss or change to the fiber's microstructure. Combined with Table 2, it can be seen that the diffraction angles corresponding to the characteristic peaks in the XRD graph have basically not changed. In summary, it can be shown that grafting modification on the surface of cotton fabrics does not change the crystal type.
[0070]
[0071] The AFM test was performed on the cotton surface after secondary modification, and the results are as follows Fig.14 As shown in Figure 2. As we all know, the surface of unmodified cotton fabric is smooth and has no obvious rough structure. After secondary modification, the surface of cotton fabric has obvious rough structure, such as Fig.14 The AFM test combined with the EDS results shows that the micro-nano rough structure on the surface of cotton fabric and the low surface energy substances on the surface together give it excellent hydrophobic properties.
[0072] Example 2 Oil-water separation and self-cleaning performance of cotton fabric after secondary modification
[0073] The self-cleaning and oil-water separation performance of cotton fabrics modified with perfluoropolyether carboxylic acid (PS-PFPE) were tested. Methylene blue and chalk ash simulants were used as pollutants, such as Fig.15 As shown in (b) and (c), when the fabric surface is rinsed with water droplets, the water droplets quickly roll over the fabric surface and take away the dirt. The fabric surface is free of dirt and will not be wetted. The above results show that cotton-PS-PFPE not only has hydrophobic properties, but also has self-cleaning properties. Fig.15 (a) is a diagram of the oil-water separation process of modified cotton fabric, with methylene blue aqueous solution and oil red dyed n-heptane as oil agents. It can be seen that n-heptane quickly passes through the cotton fabric under the action of gravity, while the methylene blue aqueous solution is "blocked" by the cotton fabric above due to its surface hydrophobicity, which shows that the grafted modified cotton fabric has excellent oil-water separation performance. The separation efficiency was tested, such as Fig.15 (d) shows the efficiency of grafted modified cotton fabric after 10 oil-water separation cycles. After 10 cycles, its efficiency dropped from the initial 99.5% to 98.6%, and it still has good oil-water separation performance. These results all show that the grafted modified cotton fabric has good oil-water separation and self-cleaning properties.
[0074] Example 3 Cotton fabric whiteness test, air permeability and tensile fracture test
[0075] The air permeability of cotton fabrics before and after grafting modification was tested, and the results showed that the air permeability of raw cotton was 385.2 mm / s, and that of cotton-PS-PFPE was 345.4 mm / s.
[0076] Comparative Example 1 Cotton-Br Direct Secondary Modified Fabric (Cotton-PFPE)
[0077] Take cotton-Br (according to the method of Example 1, 1.0 g), add 2.2 g of perfluoropolyether carboxylic acid with a number average molecular weight of 750, 30.0 g of toluene and 30.0 g of 1,3-bis(trifluoromethyl)benzene, then seal the device, evacuate, and pass nitrogen protection. After the perfluoropolyether carboxylic acid is completely dissolved, 148 mg of DBU is added, and then reacted at 90°C for 12 h; after the reaction is completed, the fabric is repeatedly washed three times in anhydrous methanol and ethanol, and then dried in a vacuum oven to obtain cotton-Br secondary modified fabric (cotton-PFPE).
[0078] Referring to the above method, the secondary modification time of perfluoropolyether carboxylic acid was extended to 12h, 16h and 24h to obtain different finished cotton fabrics (cotton-PFPE). The water contact angles of the four types of cotton-PFPE were measured to be 135.5±1.1º, 135.8±1.6º, 138.1±0.9º and 138.5±1.3º, respectively. It can be seen that the hydrophobic effect of directly coupling on the fiber surface and introducing perfluoropolyether chains to modify the fabric is not ideal and is far from reaching the super-hydrophobic level.
[0079] Comparative Example 2 Preparation and hydrophobic properties of conventional chemically grafted PS cotton secondary modified fabric (cotton-MPFFE)
[0080] 1.0 g (4 mmol) of initiator 4,4'-azobis(4-cyanopentanol (ACP) was added to the reaction flask, dissolved in 4.5 mL of ultra-dry THF, and placed in a constant pressure dropping funnel for use. 20.8 g (200 mmol) of styrene was added to a three-necked flask equipped with a magnetic stirrer, dissolved in 50 mL of THF, heated to 75 °C, and 1.0 g of cut cotton fabric was added. Then, the ACP solution prepared in advance was added dropwise. After the addition was completed, the grafting reaction was carried out for 5 h. After the reaction was completed, the cotton cloth was washed three times in anhydrous ethanol, then placed in a vacuum oven at 45 °C and dried to obtain cotton-M.
[0081] In another three-necked flask, add cotton fabric Cotton-M and 50 g of ultra-dry tetrahydrofuran, add 1.24 mL of ultra-dry triethylamine, and 0.45 g of 4-dimethylaminopyridine, place the three-necked flask in an ice bath, cool to 10°C, evacuate, and under nitrogen protection, drop 1.15 mL of 2-bromoisobutyryl bromide, drop it in 10 minutes, keep it at 10°C for 2 h, and then transfer it to an oil bath pot at 35°C for 24 h. After the reaction, wash the cotton cloth in anhydrous ethanol three times, then place it in a vacuum oven at 45°C and dry it to obtain Cotton-MBr.
[0082] Take the cotton-MBr prepared above, add 2.1 g of perfluoropolyether carboxylic acid with a number average molecular weight of 750, 30.0 g of toluene and 30.0 g of 1,3-bis(trifluoromethyl)benzene, then seal the device, evacuate, and pass nitrogen protection. After the perfluoropolyether carboxylic acid is completely dissolved, 150 mg of DBU is added, and then reacted at 90°C for 12 h; after the reaction is completed, the fabric is repeatedly washed three times in anhydrous methanol and ethanol, and then dried in a vacuum oven to obtain cotton-MBr secondary modified fabric (cotton-MPFPE).
[0083] Referring to the above method, the secondary modification time of perfluoropolyether carboxylic acid was changed to 16h and 24h, and different finished cotton fabrics (cotton-MPFPE) were obtained. The water contact angles of three kinds of cotton-PFPE with the secondary modification time of perfluoropolyether carboxylic acid of 8h, 16h and 24h were measured to be 138.6±1.3º, 137.9±1.0º and 140.1±1.3º respectively. Since cotton fabrics were treated according to the traditional grafting modification method, the polystyrene polymers connected to the fiber surface formed a film layer covering ( Fig.16 ), and the rough morphology of the base cannot be constructed, and the hydrophobic effect of the prepared perfluoropolyether modified fabric cannot achieve the superhydrophobic function with a water contact angle higher than 150°.
[0084] summary
[0085] The present invention reacts the cotton fabric after alkalization treatment with 2-bromoisobutyryl bromide, and then initiates the grafting of styrene on the cotton fabric in a heterogeneous system under the initiation conditions of PMDETA / CuBr, giving the cotton fabric a rough morphology. Using the C-Br bond, PFPE-COOH with different molecular weights is used for secondary modification under the catalysis of DBU. The modification results under different conditions are characterized by SEM, EDS, and FT-IR, and the surface elements of the cotton fabric before and after modification are tested by XPS. The results show that by giving the cotton fabric a low surface energy substance, the hydrophobic property of the material surface can be improved. After the secondary modification of perfluoropolyether carboxylic acids with different molecular weights, the water contact angle of the fabric is increased from 144.8±3.6° to 152.3±1.7° and 155.2±3.5° respectively.
[0086] The modified cotton fabric was further tested for oil-water separation and self-cleaning. The test showed that it had good oil-water separation and self-cleaning effects. After 10 oil-water separation cycle tests, the separation efficiency of the modified fabric remained above 98%. The TGA test showed that the heat resistance of the modified cotton fabric was improved. The cotton fabric before and after modification was analyzed using XRD. The test results showed that there was no significant change in XRD before and after modification. The air permeability of the cotton fabric before and after grafting modification was tested, and it was found that the air permeability could be well maintained.
Claims
1. A method for preparing a super-hydrophobic cotton fabric modified by controlled grafting of styrene. It is characterized in that The method comprises the following steps: reacting a bromine source with cotton fabric to obtain cotton-Br; then reacting styrene with cotton-Br to obtain cotton-PS; then reacting cotton-PS with perfluoropolyether carboxylic acid to obtain a controllably grafted styrene secondary modified super-hydrophobic cotton fabric; the bromine source is an organic bromine compound; the mass ratio of the bromine source to the cotton fabric is (0.5-2.5):1; the temperature of the reaction of the bromine source with the cotton fabric is 5-45°C, and the reaction time is 5-30 hours.
2. The method for preparing the super-hydrophobic cotton fabric modified by controlled grafting styrene according to claim 1, It is characterized in that The reaction between the bromine source and the cotton fabric is carried out in the presence of an organic base and an organic catalyst; the amount of the organic catalyst used is 1 to 8% of the mass of the cotton fabric.
3. The method for preparing the super-hydrophobic cotton fabric modified by controlled grafting styrene according to claim 1, It is characterized in that The reaction of styrene and cotton-Br is carried out in an organic solvent; when styrene and cotton-Br react, the concentration of styrene is 0.1-1 mol / L; when styrene and cotton-Br react, the bath ratio is 1:(50-150).
4. The method for preparing the super-hydrophobic cotton fabric modified by controlled grafting styrene according to claim 1, It is characterized in that The reaction of styrene and cotton-Br is carried out in the presence of an organic ligand and a copper salt; the mass ratio of cotton-Br, organic ligand and copper salt is 1:(0.8-1.2):(1-1.5); the reaction temperature of styrene and cotton-Br is 30-100°C; and the reaction time is 5-30 hours.
5. The method for preparing the super-hydrophobic cotton fabric modified by controlled grafting styrene secondary according to claim 1, It is characterized in that The reaction of cotton-PS and perfluoropolyether carboxylic acid is carried out under the catalysis of an organic base; the mass ratio of cotton-PS, perfluoropolyether carboxylic acid and organic base is 1:(1.5-3):(0.1-0.2).
6. The method for preparing the super-hydrophobic cotton fabric modified by controlled grafting of styrene according to claim 1, It is characterized in that The reaction temperature of cotton-PS and perfluoropolyether carboxylic acid is 80-100° C. and the reaction time is 10-15 hours.
7. The super-hydrophobic cotton fabric secondarily modified with controllable grafted styrene is prepared according to the method for preparing the super-hydrophobic cotton fabric secondarily modified with controllable grafted styrene according to claim 1.
8. Use of the controllably grafted styrene-secondarily modified super-hydrophobic cotton fabric according to claim 7 in the preparation or as a hydrophobic material.
9. Use of the controllably grafted styrene-secondarily modified super-hydrophobic cotton fabric according to claim 7 in the preparation or as an oil-water separation material.