A sodium-modified zeolite adsorbent and a method for reducing sodium ion concentration in lithium-rich solution

Through the use of sodium modified zeolite adsorbent, the adsorption selectivity under different temperature and pH conditions is used to solve the problem of sodium ion removal in lithium-rich liquid, realize a low energy consumption and recyclable process, and improve the lithium-sodium ratio and The simplicity of crystallizing lithium.

CN116440857BActive Publication Date: 2024-10-18LIS (SHANGHAI) MATERIALS TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310286373.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-18
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

In the existing technology, it is difficult to remove sodium ions from lithium-rich liquids with low energy consumption without losing lithium ions, which affects the crystallization lithium precipitation effect and process efficiency.

Method used

The sodium modified zeolite adsorbent is used to modify the analcite with saturated sodium sulfate, and combined with the adsorption selectivity under different temperature and pH conditions, the low energy consumption of sodium ions and lithium ions in the lithium-rich liquid is achieved.

Benefits of technology

It effectively reduces the sodium ion concentration in the lithium-rich liquid, increases the lithium-to-sodium ratio, and simplifies the subsequent crystallization lithium precipitation process. The process is recyclable and does not require water washing and impurity discharge.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116440857B_ABST
    Figure CN116440857B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of adsorption materials, and specifically relates to a sodium-modified zeolite adsorbent and a method for reducing the sodium ion concentration in a lithium-rich solution. The sodium-modified zeolite adsorbent provided by the present invention, after the analcime is modified with saturated sodium sulfate, can show different adsorption selectivity for lithium ions and sodium ions in the lithium-rich solution under different temperatures and different pH conditions, thereby realizing a low-energy, recyclable process to continuously remove sodium ions from a high-sodium, high-lithium solution. The lithium-sodium ratio in the lithium-rich solution can be increased to 2.5:1 or even 3:1, and the subsequent concentrated crystallization lithium precipitation process becomes very simple.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adsorption materials, and in particular relates to a sodium-modified zeolite adsorbent and a method for reducing the sodium ion concentration in lithium-rich liquid. Background Art

[0002] Lithium and lithium salts can be widely used in energy, metallurgy, chemical industry and other fields. Lithium is an indispensable raw material to support the development of new energy vehicle industry.

[0003] The lithium reserves in salt lake brine account for more than 70% of the total lithium reserves. In addition, the process of extracting lithium from salt lake brine is relatively simple and the cost is relatively low. Therefore, extracting lithium from salt lake brine has become the main mining method in the industry. The process of extracting lithium from salt lake brine usually includes extraction, ion exchange adsorption, electrodialysis, and electro-deintercalation. Since the lithium content in brine is extremely low, the purification process of salt lake brine is an indispensable process.

[0004] Lithium ion screen adsorption technology is a low-cost, environmentally friendly, efficient, and rapidly scalable salt lake brine lithium extraction technology. After the lithium ion screen adsorbs lithium ions from the salt lake brine, the adsorbed lithium ions need to be resolved into the analytical solution through an analytical process. After the analytical solution is concentrated, sodium hydroxide is added to adjust the pH to above 12 to filter out calcium and magnesium ions. At this time, the lithium-rich solution mainly contains lithium ions, sodium ions (added in large quantities when adjusting the pH), and sulfate ions. The presence of a large amount of sodium ions makes it difficult to further concentrate the lithium-rich solution, resulting in high energy consumption, and will also affect the effect of the final crystallization of lithium.

[0005] In the prior art, the sodium ions in the lithium-rich liquid of the sulfuric acid system can be removed by crystallizing Glauber's salt after freezing, but the energy consumption is high and some lithium ions will be lost during solid-liquid separation. The sodium ions in the lithium-rich liquid of the chloride system cannot be removed and can only be circulated or discharged with the mother liquor after crystallization and lithium precipitation, resulting in a large amount of lithium ions being lost with the mother liquor.

[0006] In view of this, how to remove sodium ions from lithium-rich liquid in a low-energy manner without losing lithium ions is a major challenge faced in the field. Summary of the invention

[0007] Therefore, the technical problem to be solved by the present invention is to overcome the above-mentioned defects in the prior art, thereby providing a sodium-modified zeolite adsorbent and a method for reducing the sodium ion concentration in a lithium-rich solution.

[0008] To this end, the present invention provides the following technical solutions:

[0009] The invention provides a sodium modified zeolite adsorbent, which is modified by using analcime as raw material and subjected to saturated sodium sulfate treatment.

[0010] Optionally, the modification treatment is to boil the analcime in a saturated sodium sulfate solution for 2-4 hours.

[0011] Optionally, the modification process is repeated 3-6 times, and the turbid liquid is poured off after each modification process is completed.

[0012] Optionally, the usage ratio of the saturated sodium sulfate solution to analcime is 3-20 mL / g.

[0013] Optionally, the particle size of the analcime is 30-40 mesh.

[0014] The present invention also provides a method for reducing the sodium ion concentration in lithium-rich liquid, using the sodium-modified zeolite adsorbent to perform adsorption treatment on the lithium-rich liquid.

[0015] Optionally, the method for reducing the sodium ion concentration in the lithium-rich solution comprises the following steps:

[0016] S1, adjusting the pH of the lithium-rich solution to 11-12.5;

[0017] S2, contacting the lithium-rich liquid with the sodium-modified zeolite adsorbent at a flow rate of 1-5 times the volume of the adsorbent per hour for a contact time of 2-5 hours to obtain a sodium-free lithium-rich liquid.

[0018] Optionally, the adsorption temperature is 10-60°C.

[0019] Optionally, the sodium-modified zeolite adsorbent after adsorption is subjected to analytical treatment;

[0020] Optionally, a solution with a pH of 1.5-2 and containing 0.05-0.3 mol / L lithium sulfate is used for analysis; optionally, a lithium ion sieve analysis solution is used for analysis.

[0021] Optionally, the lithium ion sieve analytical solution is brought into contact with the adsorbed sodium-modified zeolite adsorbent at a flow rate of 5-10 times the adsorbent volume / hour, and the contact time is 0.5-1 h.

[0022] Specifically, the preparation of the sodium modified zeolite is as follows: analcime is taken, ground into 30-40 meshes, placed in a saturated sodium sulfate solution and boiled for 2-4 hours, and the turbid liquid is poured off, and this process is repeated 3-6 times. After the zeolite modification is completed, it is dried and placed in an adsorption device.

[0023] Specifically, if Figure 1 As shown, the detailed operation method for reducing the sodium ion concentration in the lithium-rich solution can be:

[0024] The lithium-rich solution with a lithium ion concentration of about 10g / L, a sodium ion concentration of more than 10g / L, a pH of about 12.0, and anions mainly composed of sulfate ions, is passed through an adsorption tower equipped with a sodium-modified zeolite adsorbent at room temperature or after heating at a flow rate of 1-5 times the adsorbent volume / hour, and the adsorption is completed after 2-5 hours. Since the adsorption selectivity of sodium-modified zeolite for hydrated sodium ions is much higher than that for hydrated lithium ions at 10-60°C and pH=11-12.5, the lithium ion concentration in the sodium-removed lithium-rich solution after adsorption is still about 10g / L, and the sodium ion concentration is not higher than 5g / L. The lithium-rich solution only needs to be simply concentrated to crystallize and precipitate lithium.

[0025] Since sulfate, sodium ions, and lithium ions are all valuable ions, there is no need to wash with water, and the sodium-type zeolite can be directly analyzed after adsorption. After using a lithium sulfate solution or lithium ion sieve analysis solution with a pH of about 1.5-2.0, 0.05-0.3 mol / L (i.e., the analysis solution obtained by using sulfuric acid analysis in the lithium ion sieve adsorption method for lithium extraction from salt lakes, hereinafter referred to as "lithium ion sieve analysis solution"), it is passed into the adsorption tower and circulated at a flow rate of 5-10 times the adsorbent volume / hour, and the analysis is completed in 0.5-1 hour. Since the lithium ion concentration in the lithium ion sieve analysis solution is higher than the sodium ion concentration, and the selectivity of the sodium-modified zeolite for hydrated sodium ions and hydrated lithium ions is not much different in an environment of pH = 1.5-2.0, a large amount of sodium ions are replaced by hydrogen ions and lithium ions from the zeolite. After the analysis of the zeolite is completed, the lithium ion sieve analysis solution becomes a zeolite analysis solution, in which the lithium ion concentration is reduced, the sodium ion concentration is greatly increased, and the pH is increased. The effective sites in the sodium-modified zeolite are occupied by hydrogen ions and lithium ions, which will be exchanged with sodium ions in the subsequent adsorption, and the lithium ions will enter the next round of lithium-rich solution for utilization.

[0026] After obtaining the zeolite analysis solution, the zeolite analysis solution is mixed with the lithium ion sieve analysis solution at a ratio of 1:1-1:5, and the sodium zeolite that has been adsorbed can be analyzed again. After the above analysis is completed, the sodium ion concentration in the zeolite analysis solution is much higher than the lithium ion concentration. When the sodium ion concentration in the zeolite analysis solution is ≥10g / L, it is simply concentrated to a sodium ion concentration of 30-40g / L and then frozen to below -10°C. A large amount of sodium sulfate decahydrate crystals precipitate. By centrifugation, sodium sulfate decahydrate solid and a solution that can be used in the above analysis step after dilution can be obtained. Through this method, the sodium ions that are continuously enriched in the system can be stripped out of the system, thereby ensuring that the system itself can be recycled.

[0027] Typically, sodium sulfate decahydrate can be used to produce 0.5-2 mol / L sulfuric acid solution and 0.5-2 mol / L sodium hydroxide solution through bipolar membrane electrodialysis. The sulfuric acid solution can be used to desorb the lithium ion sieve adsorbent, and the sodium hydroxide solution can be used to adjust the pH value of the lithium ion sieve desorption solution after further concentration. At this point, all impurities have completed the cycle in the system without external discharge. The lithium-sodium ratio in the lithium-rich solution is increased to 2.5:1 or even 3:1, and the subsequent concentration and crystallization lithium precipitation process becomes very simple.

[0028] The technical solution of the present invention has the following advantages:

[0029] 1. The sodium-modified zeolite adsorbent provided by the present invention, after the analcime is modified by saturated sodium sulfate, can show different adsorption selectivity for lithium ions and sodium ions in lithium-rich solution under different temperatures and different pH conditions, thereby realizing the continuous removal of sodium ions from high-sodium and high-lithium solutions in a low-energy, recyclable process.

[0030] 2. The method for reducing the sodium ion concentration in the lithium-rich solution provided by the present invention utilizes the different adsorption selectivity of sodium-modified zeolite for lithium ions and sodium ions in the lithium-rich solution under different temperatures and different pH conditions, and continuously removes sodium ions from the high-sodium and high-lithium solution in a low-energy, recyclable process. The lithium-sodium ratio in the lithium-rich solution can be increased to 2.5:1 or even 3:1, and the subsequent concentration, crystallization and lithium precipitation process becomes very simple. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0032] Figure 1 This is a specific operation process for reducing the sodium ion concentration in lithium-rich solution provided by the present invention. DETAILED DESCRIPTION

[0033] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0034] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0035] In order to facilitate the comparison between data, the lithium-rich solution and lithium ion sieve analysis solution used in the following examples of the present invention are all from the lithium extraction process of brine from JZCK Salt Lake in Tibet, and their specific compositions are shown in the following table:

[0036] Table 1

[0037]

[0038] Analcime was provided by Lingshou County Ningbo Mineral Products Co., Ltd.

[0039] Example 1

[0040] A sodium-modified zeolite adsorbent and a method for reducing the sodium ion concentration in a lithium-rich solution, wherein the specific operation is as follows:

[0041] Preparation of sodium-modified zeolite: Take 40g of analcime, grind it to 30-40 mesh, place it in 120ml of saturated sodium sulfate solution and boil it for 4 hours, pour off the turbid liquid, repeat this process 3 times, the zeolite modification is completed, and place it in an adsorption device after drying.

[0042] Method of operation to reduce the sodium ion concentration in lithium-rich solution:

[0043] The lithium-rich solution was passed through an adsorption tower filled with sodium-modified zeolite adsorbent at a flow rate of 5 times the adsorbent volume / hour at room temperature of 15°C, and the adsorption was completed after 2 hours.

[0044] After adsorption, the lithium ion concentration in the sodium-removed lithium-rich liquid is 9.7 g / L, and the sodium ion concentration is 4 g / L.

[0045] Example 2

[0046] A sodium-modified zeolite adsorbent and a method for reducing the sodium ion concentration in a lithium-rich solution, wherein the specific operation is as follows:

[0047] Preparation of sodium-modified zeolite: Take 40g of natural analcime, grind it to 30-40 mesh, place it in 800ml of saturated sodium sulfate solution and boil it for 2 hours, pour off the turbid liquid, repeat this process 6 times, the zeolite modification is completed, and place it in an adsorption device after drying.

[0048] Method of operation to reduce the sodium ion concentration in lithium-rich solution:

[0049] After the lithium-rich solution was heated to 45°C, it was passed through an adsorption tower filled with sodium-modified zeolite adsorbent at a flow rate of 1 times the adsorbent volume / hour. The adsorption was completed after 5 hours.

[0050] After adsorption, the lithium ion concentration in the sodium-removed lithium-rich liquid is 9.8 g / L, and the sodium ion concentration is 3.3 g / L.

[0051] Example 3

[0052] A sodium-modified zeolite adsorbent and a method for reducing the sodium ion concentration in a lithium-rich solution, wherein the specific operation is as follows:

[0053] Preparation of sodium-modified zeolite: Take 40g of natural analcime, grind it to 30-40 mesh, place it in 400ml of saturated sodium sulfate solution and boil it for 3 hours, pour off the turbid liquid, repeat this process 4 times, the zeolite modification is completed, and place it in an adsorption device after drying.

[0054] Method of operation to reduce the sodium ion concentration in lithium-rich solution:

[0055] After the lithium-rich solution was heated to 50°C, it was passed through an adsorption tower filled with sodium-modified zeolite adsorbent at a flow rate of 3 times the adsorbent volume / hour. The adsorption was completed after 4 hours.

[0056] After adsorption, the lithium ion concentration in the sodium-removed lithium-rich solution is 10.0 g / L, and the sodium ion concentration is 3.4 g / L.

[0057] Example 4

[0058] A sodium-modified zeolite adsorbent and a method for reducing the sodium ion concentration in a lithium-rich solution, wherein the specific operation is as follows:

[0059] Preparation of sodium-modified zeolite: Take 40g of natural analcime, grind it to 30-40 mesh, place it in 200ml of saturated sodium sulfate solution and boil it for 3 hours, pour off the turbid liquid, repeat this process 5 times, the zeolite modification is completed, and place it in an adsorption device after drying.

[0060] like Figure 1 As shown, the detailed operation method for reducing the sodium ion concentration in the lithium-rich solution is:

[0061] After the lithium-rich liquid is heated to 50°C, it is passed through an adsorption tower equipped with a sodium-modified zeolite adsorbent at a flow rate of 2 times the adsorbent volume / hour. The adsorption is completed after 4 hours. The lithium ion concentration in the sodium-free lithium-rich liquid after adsorption is 9.9g / L, and the sodium ion concentration is 3.5g / L. The lithium-rich liquid only needs to be simply concentrated to crystallize lithium.

[0062] After the adsorption is completed, the sodium-type zeolite can be directly analyzed. After the lithium ion sieve analysis solution is passed into the adsorption tower, it is circulated and analyzed at a flow rate of 5 times the adsorbent volume / hour, and the analysis is completed in 1 hour. After the zeolite analysis is completed, the lithium ion sieve analysis solution becomes a zeolite analysis solution, in which the lithium ion concentration is 1.3g / L, the sodium ion concentration is 5.6g / L, and the pH is 2.0. The effective sites in the sodium-modified zeolite are occupied by hydrogen ions and lithium ions, which will be exchanged with sodium ions in the subsequent adsorption, and the lithium ions will enter the next round of lithium-rich solution for utilization.

[0063] After obtaining the zeolite analysis solution, the zeolite analysis solution is mixed with the lithium ion sieve analysis solution at a ratio of 1:1, and the adsorbed sodium zeolite can be analyzed again. After repeated use for 4 times, the sodium ion concentration in the zeolite analysis solution is 10.2g / L. After simply concentrating it to a sodium ion concentration of 30g / L and freezing it to -10°C, a large amount of sodium sulfate decahydrate crystals are precipitated. Through centrifugal separation, sodium sulfate decahydrate solid and a solution that can be used in the above analysis step after dilution can be obtained.

[0064] The sodium sulfate decahydrate can be used to produce 1 mol / L sulfuric acid solution and 1 mol / L sodium hydroxide solution by bipolar membrane electrodialysis. The sulfuric acid solution can be used to desorb the lithium ion sieve adsorbent, and the sodium hydroxide solution can be used to adjust the pH value of the lithium ion sieve desorption solution after further concentration.

[0065] Example 5

[0066] A sodium-modified zeolite adsorbent and a method for reducing the sodium ion concentration in a lithium-rich solution, wherein the specific operation is as follows:

[0067] Preparation of sodium-modified zeolite: Take 40g of natural analcime, grind it to 30-40 mesh, place it in 200ml of saturated sodium sulfate solution and boil it for 3 hours, pour off the turbid liquid, repeat this process 5 times, the zeolite modification is completed, and place it in an adsorption device after drying.

[0068] like Figure 1 As shown, the detailed operation method for reducing the sodium ion concentration in the lithium-rich solution is:

[0069] After the lithium-rich liquid is heated to 50°C, it is passed through an adsorption tower equipped with a sodium-modified zeolite adsorbent at a flow rate of 4 times the adsorbent volume / hour. The adsorption is completed after 4 hours. The lithium ion concentration in the sodium-free lithium-rich liquid after adsorption is 9.8g / L, and the sodium ion concentration is 3.4g / L. The lithium-rich liquid only needs to be simply concentrated to crystallize and precipitate lithium.

[0070] After the adsorption is completed, the sodium-type zeolite can be directly analyzed. After the lithium ion sieve analysis solution is passed into the adsorption tower, it is circulated and analyzed at a flow rate of 10 times the adsorbent volume / hour, and the analysis is completed in 0.5 hours. After the zeolite is analyzed, the lithium ion sieve analysis solution becomes a zeolite analysis solution, in which the lithium ion concentration is 1.5g / L, the sodium ion concentration is 5.1g / L, and the pH is 1.9. The effective sites in the sodium-modified zeolite are occupied by hydrogen ions and lithium ions, which will be exchanged with sodium ions in the subsequent adsorption, and the lithium ions will enter the next round of lithium-rich solution for utilization.

[0071] After obtaining the zeolite analysis solution, the zeolite analysis solution was mixed with the lithium ion sieve analysis solution at a ratio of 1:5, and the adsorbed sodium zeolite was analyzed again. After repeated use 82 times, the sodium ion concentration in the zeolite analysis solution was 10.1 g / L. After simply concentrating it to a sodium ion concentration of 40 g / L and freezing it to -10°C, a large amount of sodium sulfate decahydrate crystals precipitated. Through centrifugal separation, sodium sulfate decahydrate solid and a solution that can be used in the above analysis step after dilution can be obtained.

[0072] The sodium sulfate decahydrate can be used to produce 1 mol / L sulfuric acid solution and 1 mol / L sodium hydroxide solution by bipolar membrane electrodialysis. The sulfuric acid solution can be used to desorb the lithium ion sieve adsorbent, and the sodium hydroxide solution can be used to adjust the pH value of the lithium ion sieve desorption solution after further concentration.

[0073] Example 6

[0074] A sodium-modified zeolite adsorbent and a method for reducing the sodium ion concentration in a lithium-rich solution, wherein the specific operation is as follows:

[0075] Preparation of sodium-modified zeolite: Take 40g of natural analcime, grind it to 30-40 mesh, place it in 200mL of saturated sodium sulfate solution and boil it for 3 hours, pour off the turbid liquid, repeat this process 4 times, the zeolite modification is completed, and place it in an adsorption device after drying.

[0076] like Figure 1 As shown, the detailed operation method for reducing the sodium ion concentration in the lithium-rich solution is:

[0077] After the lithium-rich liquid is heated to 50°C, it is passed through an adsorption tower equipped with a sodium-modified zeolite adsorbent at a flow rate of 3.5 times the adsorbent volume / hour. The adsorption is completed after 3.5 hours. The lithium ion concentration in the sodium-free lithium-rich liquid after adsorption is 9.5g / L, and the sodium ion concentration is 3.7g / L. The lithium-rich liquid only needs to be simply concentrated to crystallize lithium.

[0078] After the adsorption is completed, the sodium-type zeolite can be directly analyzed. After the lithium ion sieve analysis solution is passed into the adsorption tower, it is circulated and analyzed at a flow rate of 8 times the adsorbent volume / hour, and the analysis is completed in 45 minutes. After the zeolite is analyzed, the lithium ion sieve analysis solution becomes a zeolite analysis solution, in which the lithium ion concentration is 1.4g / L, the sodium ion concentration is 5.4g / L, and the pH is 2.0. The effective sites in the sodium-modified zeolite are occupied by hydrogen ions and lithium ions, which will be exchanged with sodium ions in the subsequent adsorption, and the lithium ions will enter the next round of lithium-rich solution for utilization.

[0079] After obtaining the zeolite analysis solution, the zeolite analysis solution was mixed with the lithium ion sieve analysis solution at a ratio of 1:3, and the adsorbed sodium zeolite was analyzed again. After repeated use 32 times, the sodium ion concentration in the zeolite analysis solution was 9.9 g / L. After simply concentrating it to a sodium ion concentration of 35 g / L and freezing it to -10°C, a large amount of sodium sulfate decahydrate crystals precipitated. Through centrifugal separation, sodium sulfate decahydrate solid and a solution that can be used in the above analysis step after dilution can be obtained.

[0080] The sodium sulfate decahydrate can be used to produce 1 mol / L sulfuric acid solution and 1 mol / L sodium hydroxide solution by bipolar membrane electrodialysis. The sulfuric acid solution can be used to desorb the lithium ion sieve adsorbent, and the sodium hydroxide solution can be used to adjust the pH value of the lithium ion sieve desorption solution after further concentration.

[0081] Comparative Example 1

[0082] Compared with Example 1, the only difference is that the natural analcime is not treated with sodium. The lithium ion concentration in the sodium-free lithium-rich solution after adsorption is about 9.2 g / L, and the sodium ion concentration is 10.4 g / L.

[0083] Comparative Example 2

[0084] Compared with Example 1, the only difference is that the adsorption temperature is a low temperature of 0°C (not frozen). After adsorption, the lithium ion concentration in the sodium-removed lithium-rich liquid is about 10 g / L, and the sodium ion concentration is 11.3 g / L.

[0085] Comparative Example 3

[0086] Compared with Example 1, the only difference is that the adsorption temperature is room temperature 80° C. After adsorption, the lithium ion concentration in the sodium-removed lithium-rich solution is about 9.5 g / L, and the sodium ion concentration is 10.8 g / L.

[0087] Comparative Example 4

[0088] Compared with Example 1, the only difference is that saturated sodium carbonate is used instead of saturated sodium sulfate. After adsorption, the lithium ion concentration in the sodium-removed lithium-rich solution is about 8.2 g / L, and the sodium ion concentration is 8.9 g / L.

[0089] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A sodium-modified zeolite adsorbent, characterized in that: Using analcime as raw material, it is modified by saturated sodium sulfate. The modification treatment is to place the analcime in a saturated sodium sulfate solution and boil it for 2-4 hours.

2. The sodium-modified zeolite adsorbent according to claim 1, characterized in that: The modification process is repeated 3-6 times, and the turbid liquid is poured off after each modification process is completed.

3. The sodium-modified zeolite adsorbent according to claim 1, characterized in that: The usage ratio of the saturated sodium sulfate solution to analcime is 3-20 mL / g.

4. The sodium-modified zeolite adsorbent according to any one of claims 1 to 3, characterized in that: The particle size of the analcime is 30-40 meshes.

5. A method for reducing the sodium ion concentration in a lithium-rich solution, characterized in that: Adsorbing the lithium-rich liquid using the sodium-modified zeolite adsorbent according to any one of claims 1 to 4; The pH of the adsorption treatment is 11-12.5, and the adsorption temperature is 10-60°C.

6. The method for reducing the sodium ion concentration in lithium-rich solution according to claim 5, characterized in that: The following steps are involved: S1, adjusting the pH of the lithium-rich solution to 11-12.5; S2, contacting the lithium-rich liquid with the sodium-modified zeolite adsorbent at a flow rate of 1-5 times the volume of the adsorbent per hour for a contact time of 2-5 hours to obtain a sodium-free lithium-rich liquid.

7. The method for reducing the sodium ion concentration in lithium-rich solution according to claim 6, characterized in that: The sodium-modified zeolite adsorbent after adsorption was subjected to analytical treatment.

8. The method for reducing the sodium ion concentration in lithium-rich solution according to claim 7, characterized in that: The analytical treatment is performed using a solution having a pH of 1.5-2 and containing 0.05-0.3 mol / L lithium sulfate.

9. The method for reducing the sodium ion concentration in lithium-rich solution according to claim 7, characterized in that: Lithium ion sieve analytical solution was used for analytical treatment.

10. The method for reducing the sodium ion concentration in lithium-rich solution according to claim 9, characterized in that: The lithium ion sieve analytical solution is contacted with the adsorbed sodium modified zeolite adsorbent at a flow rate of 5-10 times the adsorbent volume / hour, and the contact time is 0.5-1h.

Citation Information

Patent Citations

  • Method for modifying natural zeolite powder

    CN101569852A

  • Technology for preparing potash fertilizer from potassium feldspar-decomposed mother liquor employing adsorption method

    CN103864472A

  • Integrated technology and equipment for bitter bittern resource utilization

    CN105692656A

  • Ion sieve type sodium ion adsorbent and method for removing impurity sodium in lithium chloride

    CN105833830A

  • Carbon dioxide adsorbent, carbon dioxide adsorption tower and carbon dioxide recovery system

    CN107115845A