A bismuth tungstate-bismuth vanadate composite catalyst and its preparation method and application
By constructing a bismuth tungstate-bismuth vanadate composite catalyst, combining piezoelectric and photocatalytic characteristics, using natural light and mechanical vibration, the problems of low efficiency and high cost of semiconductor photocatalytic technology are solved, and the efficient synthesis of H2O2 and degradation of rhodamine B are achieved. Effect.
Patent Information
- Application Number
- CN202310285482.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-03-22
AI Technical Summary
The existing semiconductor photocatalytic technology has low quantum efficiency and high preparation cost when synthesizing advanced oxides (H2O2), making it difficult to meet actual needs.
Through morphological engineering, bismuth tungstate-bismuth vanadate composite catalyst was constructed, combined with the advantages of piezoelectric materials and photocatalysts, and single-layer sheet-like bismuth tungstate was prepared by KBr or CTAB assisted bottom-up method, and quantums were grown on it. Bismuth vanadate forms a bismuth tungstate-bismuth vanadate composite catalyst, which is catalyzed using natural light and mechanical vibration.
It realizes a catalyst with low cost, easy preparation, unique structure, large specific surface area and short carrier transport distance, and can efficiently catalyze the synthesis of H2O2 and degradation of rhodamine B, suitable for large-scale production, and green and recyclable materials.
Smart Images

Figure CN116440895B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of catalytic technology, and in particular to a bismuth tungstate-bismuth vanadate composite catalyst and a preparation method and application thereof. Background Art
[0002] Hydrogen peroxide (H2O2) is a green oxidant used in bleaching, sterilization, sewage treatment and organic synthesis. The domestic market demand for H2O2 is increasing. However, the current method for synthesizing H2O2 is mainly the anthraquinone method, which has high equipment requirements, high energy consumption and harms the environment. Therefore, it is imperative to develop a new method for synthesizing H2O2 that is environmentally friendly and low in energy consumption.
[0003] Photocatalytic advanced oxidation is a very promising method for synthesizing H2O2. However, conventional semiconductor photocatalytic advanced oxidation technology has low quantum efficiency (<10%), making it difficult to meet the actual needs of production and life. Therefore, it is necessary to try to improve the activity of semiconductor photocatalytic reactions. Piezoelectric materials can induce piezoelectric polarization charges under external stress and generate surface piezoelectric potential. On the one hand, this piezoelectric potential can serve as a reaction driving force to induce surface interface redox catalytic reactions. On the other hand, the built-in electric field induced by the piezoelectric potential can promote the directional separation and transfer of photogenerated charges. Combining piezoelectric materials with narrow bandgap semiconductors or metal nanoparticles is a way to make up for the inherent defects of piezoelectric materials such as poor photoresponse performance, electrical conductivity, and low carrier concentration. For example, Shi et al. (Nano Energy 2020, 69, 104448) decorated BiVO4 quantum dots on ZnO nanorods to construct a piezoelectric potential-assisted photocatalyst. The results show that the efficiency of formaldehyde degradation under mechanical stimulation is significantly improved by optimizing the BiVO4 quantum dot-decorated ZnO nanorod array. Yan et al. (Applied Catalysis B: Environmental 2019, 259, 118084) prepared Au nanoparticles modified BiVO4 (Au / BiVO4), Au / BiVO4 bifunctional piezoelectric catalyst, which significantly improved the ·OH generation rate and H2O2 accumulation. Although the above method can improve the performance of the catalyst to a certain extent, the preparation cost is high. Although BiVO4 has good absorption of visible light, the diffusion length of photogenerated holes in BiVO4 is less than 50nm, which limits the thickness of the photocatalytic layer, resulting in poor photogenerated charge separation ability, and most of them are recombined before reaching the catalyst surface. Studies have shown that the two-dimensional layered structure Bi2WO6 can form a heterostructure through the stacking of chemical bonds between layers and form a built-in electric field, enhance charge separation, and even induce a new band structure, with excellent piezoelectric properties (Nature Communications 2015, 6, 8340). At the same time, ultra-thin layered two-dimensional materials also have flexoelectricity and higher polarization potential, which can inhibit the recombination of carriers and accelerate their separation and transfer. Considering the advantages of heterojunction and the unique structure of bismuth-based semiconductors, it is desirable to construct a perfect heterojunction between two bismuth-based semiconductors with very similar crystal structures. Therefore, using morphological engineering to combine piezoelectric materials with specific structures and morphologies with photocatalytic materials is an important method to improve the performance of catalysts.
[0004] In view of the above problems, it is very meaningful and necessary to use morphological engineering to develop a catalyst that can simultaneously utilize light and mechanical vibration, has low preparation cost, is non-toxic and harmless, and is highly efficient in catalytic synthesis of H2O2 and degradation of Rhodamine B to truly meet the needs of actual development. Summary of the invention
[0005] The purpose of the present invention is to provide a bismuth tungstate-bismuth vanadate composite catalyst and its preparation method and application in order to overcome the defects of the above-mentioned prior art. The unique structure of the catalyst is constructed through morphological engineering, combining the advantages of piezoelectric materials and photocatalysts, and has the advantages of low cost, easy preparation, unique structure, large specific surface area, many contact sites, short carrier transport distance, etc. The preparation steps are simple and energy consumption is low, and large-scale production is possible. The material is green and recyclable, and can be used for catalytic synthesis of H2O2 and degradation of rhodamine B.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] The first object of the present invention is to provide a method for preparing a bismuth tungstate-bismuth vanadate composite catalyst, comprising the following steps:
[0008] S1. Prepare bismuth tungstate with a monolayer sheet structure by a bottom-up method assisted by KBr or cetyltrimethylammonium bromide (CTAB);
[0009] S2, growing quantum bismuth vanadate on the bismuth tungstate with a single-layer sheet structure obtained in step S1 by a hydrothermal template method to obtain a bismuth tungstate-bismuth vanadate composite catalyst.
[0010] Furthermore, the specific process of step S1 includes the following sub-steps:
[0011] S11, dissolving 2-6 mmol of bismuth nitrate pentahydrate (Bi(NO3)3·5H2O) in 1-2 M dilute nitric acid or ethylene glycol solution and stirring to obtain a clear solution;
[0012] S12, add 1-3 mmol sodium tungstate dihydrate (Na2WO4·2H2O) and 0.05-0.15 g KBr or add 1-3 mmol sodium tungstate dihydrate (Na2WO4·2H2O) and 0.05-0.15 g CATB to the clear solution obtained in step S11, stir evenly and transfer to a high-pressure reactor, react at 120-180° C. for 24-36 hours, and obtain the monolayer flaky bismuth tungstate by centrifugation and washing.
[0013] Further preferably, in step S11, the added amount of bismuth nitrate pentahydrate (Bi(NO3)3·5H2O) is 2 mmol.
[0014] Further preferably, in step S12, the reaction temperature is 120-140°C.
[0015] Furthermore, the specific process of step S2 includes the following sub-steps:
[0016] S21, dissolving 0.48-0.72 g of bismuth nitrate pentahydrate (Bi(NO3)3·5H2O) in 1 M dilute nitric acid or ethylene glycol solution and stirring to obtain a clear solution;
[0017] S22, adding 0.12-0.18 g of ammonium metavanadate (NH4VO3) to the clear solution obtained in step S21, stirring evenly, adding 0.2-0.8 g of silica gel and continuing to stir, then adding 2-3 g of the bismuth tungstate with the single-layer sheet structure, stirring evenly, drying, and calcining at 400-600° C. to obtain a powder;
[0018] S23, adding the powder obtained in step S22 to deionized water for ultrasonic dispersion and then transferring it into a high-pressure reactor, reacting at 180-200° C. for 24-48 hours, centrifugally washing, and drying at 60-80° C. to obtain in-situ growth of nano-sized quantum bismuth vanadate on the bismuth tungstate with a single-layer sheet structure, thereby obtaining the bismuth tungstate-bismuth vanadate composite catalyst.
[0019] More preferably, in step S23, the reaction temperature is 180°C.
[0020] The second object of the present invention is to provide a bismuth tungstate-bismuth vanadate composite catalyst, which comprises bismuth tungstate (Bi2WO6) and bismuth vanadate (BiVO4) grown thereon; the bismuth tungstate is a bismuth tungstate with a single-layer lamellar structure, and quantum bismuth vanadate (q-BiVO4) is grown on the bismuth tungstate with a single-layer lamellar structure by a hydrothermal template method; the bismuth vanadate is nano-sized.
[0021] Furthermore, the single-layer flaky structure of bismuth tungstate (Bi2WO6) is manufactured by a bottom-up method assisted by KBr or CTAB.
[0022] The third object of the present invention is to provide an application of a bismuth tungstate-bismuth vanadate composite catalyst, wherein the bismuth tungstate-bismuth vanadate composite catalyst is used to catalyze the synthesis of H2O2 or the bismuth tungstate-bismuth vanadate composite catalyst is used to degrade rhodamine B (RhB).
[0023] Furthermore, the specific process of using the bismuth tungstate-bismuth vanadate composite catalyst for catalytic synthesis of H2O2 comprises the following steps:
[0024] S311, dispersing the bismuth tungstate-bismuth vanadate composite catalyst into a beaker filled with ethanol-water solution, placing the beaker in a reaction system, and then –2 H2O2 is catalytically synthesized under the action of simulated solar light source and ultrasonic vibration frequency of 35-45kHz and power of 150-200W.
[0025] Furthermore, in step S311, the volume ratio of ethanol to water in the ethanol-water solution is 0.20-1:1; in step S311, the mass ratio of the bismuth tungstate-bismuth vanadate composite catalyst to the ethanol-water solution is 0.001-0.005:1.
[0026] Further preferably, in step S311, the power is 180W.
[0027] Furthermore, the specific process of using the bismuth tungstate-bismuth vanadate composite catalyst to degrade rhodamine B includes the following steps:
[0028] S321, dispersing 20-50 mg of the bismuth tungstate-bismuth vanadate composite catalyst into 50 ml of RhB solution with a concentration of 20-50 mg / L, stirring for 30-60 min in a dark environment, so that the RhB solution and the catalyst reach an adsorption / desorption equilibrium, and obtaining an adsorption / desorption equilibrium solution;
[0029] S322, placing the adsorption / desorption equilibrium solution obtained in step S321 under 100-150 mW cm -2 RhB was degraded under the action of simulated sunlight and ultrasonic vibration frequency of 35-45kHz and power of 150-200W. 3-6 ml of the reaction clear liquid was taken at intervals of 20-30 minutes to test the concentration of RhB by UV-visible light analyzer.
[0030] Furthermore, in step S321, the concentration ratio of the mass of the bismuth tungstate-bismuth vanadate composite catalyst to rhodamine B is 0.5-1:1.
[0031] Further preferably, in step S322, the power is 180W.
[0032] Furthermore, the catalytic reaction is carried out in an ultrasonic cleaning machine reaction system by controlling the temperature at 20-25°C through a circulating water bath. The catalytic reaction refers to the use of natural light and mechanical vibration to catalyze the synthesis of H2O2 and the degradation of rhodamine B. The catalyst of the catalytic reaction is the above-mentioned bismuth tungstate-bismuth vanadate composite catalyst.
[0033] Further preferably, the catalytic reaction is carried out in an ultrasonic cleaning machine reaction system with the temperature controlled at 25° C. by a circulating water bath.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] 1) The bismuth tungstate-bismuth vanadate composite catalyst and the preparation method thereof provided by the present invention combine the advantages of bismuth vanadate and bismuth tungstate, construct a unique structure of the catalyst through morphological engineering, and are easy to operate and mass produce.
[0036] 2) The bismuth tungstate-bismuth vanadate composite catalyst provided by the present invention has low cost, non-toxic and recyclable bismuth vanadate and bismuth tungstate.
[0037] 3) The bismuth tungstate-bismuth vanadate composite catalyst and its preparation method provided by the present invention utilize the coupling of piezoelectric materials and optical materials to improve the utilization rate of natural light and mechanical vibration. In particular, the sheet structure increases the contact area between the material and the reactant and increases the reaction sites. The ultra-thin sheet layer reduces the transport distance of the carriers and promotes the separation of photogenerated electrons and holes. The nano-sized quantum BiVO4 improves the photon efficiency. Therefore, the catalyst has great application value in the field of catalytic technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 (a) is a scanning electron microscope (SEM) image of Bi2WO6 in Comparative Example 1 of the present invention; Figure 1 (b) is a scanning electron microscope (SEM) image of q-BiVO4 in Comparative Example 2 of the present invention; Figure 1 (c) is a low-resolution transmission electron microscopy (TEM) image of the catalyst (W-0.30V) prepared in Example 1 of the present invention; Figure 1 (d) High-resolution transmission electron microscopy (TEM) image of the bismuth tungstate-bismuth vanadate composite catalyst (W-0.30V) prepared in Example 1 of the present invention.
[0039] Figure 2 These are the standard PDF card diagrams of Bi2WO6 and BiVO4 and the X-ray diffraction (XRD) diagrams of Bi2WO6 in Comparative Example 1 of the present invention, q-BiVO4 in Comparative Example 2, and W-0.30V in Example 1.
[0040] Figure 3 A comparison diagram of the effects of adding Bi2WO6, q-BiVO4 and W-0.30V to catalytically synthesize H2O2 in Application Example 1 of the present invention and Comparative Application Examples 2, 3 and 4 for comparison with the absence of catalyst in Application Example 1; wherein, a curve diagram of the change of the concentration of H2O2 catalytically synthesized by Bi2WO6, q-BiVO4 and W-0.30V under light irradiation (a), ultrasound (b), light irradiation and ultrasound (c) as a function of reaction time; Figure 3 (d) is a graph showing the concentration of H2O2 catalytically synthesized by W-0.30V changing with time under light, ultrasound, and light and ultrasound.
[0041] Figure 4A comparison diagram of the effects of adding Bi2WO6, q-BiVO4 and W-0.30V to catalytically degrade RhB in Application Example 2 of the present invention and Comparative Application Examples 2, 3 and 4 for comparison of the absence of catalyst in Application Example 1; wherein, a curve diagram of the catalytic degradation of RhB by Bi2WO6, q-BiVO4 and W-0.30V under light irradiation (a), ultrasound (b), light irradiation and ultrasound (c) versus reaction time; Figure 4 (d) is a graph showing the concentration of RhB catalytically degraded by W-0.30V over time under light, ultrasound, and light and ultrasound.
[0042] Figure 5 Schematic diagram of the structure of the bismuth tungstate-bismuth vanadate composite catalyst (W-0.30V) prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0043] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0044] Any features such as preparation methods, materials, structures or composition ratios that are not clearly described in this technical solution shall be deemed as common technical features disclosed in the prior art.
[0045] Example 1
[0046] In this embodiment, a bismuth tungstate-bismuth vanadate composite catalyst is provided. The preparation method of the bismuth tungstate-bismuth vanadate composite catalyst comprises the following steps:
[0047] (1) First, 2 mmol Bi(NO3)3·5H2O (99.0%, Sinopharm Group) was dissolved in 1 M dilute nitric acid (Sinopharm Group) or ethylene glycol (99.5%, Sinopharm Group) solution and stirred to obtain a clear solution. After adding 1 mmol Na2WO4·2H2O and 0.05 g KBr (99.0%, Sinopharm Group), the solution was stirred evenly and transferred into a high-pressure reactor and heated at 120°C for 24 h to obtain a single-layer flaky Bi2WO6 solution.
[0048] (2) 0.48 g of Bi(NO3)3·5H2O was dissolved in 1 M dilute nitric acid or ethylene glycol solution and stirred to obtain a clear solution. Then, 0.12 g of NH4VO3 (99.5%, Sinopharm Group), 0.2 g of silica gel (40%, Sinopharm Group) and 2 g of the prepared single-layer sheet structure Bi2WO6 were added to the above solution and stirred for 30 min. After the mixed solution was dried at 80°C for 12 h, the powder was placed in a porcelain boat and transferred to a muffle furnace and calcined at 400°C in air.
[0049] (3) Finally, the powder was dispersed in 70 ml of deionized water by ultrasonic treatment for 30 minutes and reacted in a reactor at 180°C for 24 hours. After naturally cooling to room temperature, the product was centrifuged and washed with deionized water several times, and then the material was dried at 80°C for 12 hours to obtain a powder as the catalyst.
[0050] The obtained catalyst powder is marked as W-0.30V, where "0.30" represents the mass ratio of the added single-layer flake-structured Bi2WO6 to Bi(NO3)3·5H2O, NH4VO3 and.
[0051] Example 2
[0052] In this embodiment, a bismuth tungstate-bismuth vanadate composite catalyst is provided. The preparation method of the catalyst is different from the preparation method in Example 1 in that: step (1) is specifically to first dissolve 6 mmol Bi(NO3)3·5H2O (99.0%, Sinopharm Group) in 2M dilute nitric acid (Sinopharm Group) or ethylene glycol (99.5%, Sinopharm Group) solution and stir to obtain a clear solution, then add 3 mmol Na2WO4·2H2O and 0.15 g KBr (99.0%, Sinopharm Group), stir evenly, transfer to a high-pressure reactor, and heat at 140°C for 36 hours to obtain a single-layer flaky structure of Bi2WO6.
[0053] Example 3
[0054] In this embodiment, a bismuth tungstate-bismuth vanadate composite catalyst is provided. The difference between the preparation method of the catalyst and the preparation method in Example 1 is that: Step (2) is specifically to dissolve 0.72g of Bi(NO3)3·5H2O in 1M dilute nitric acid or ethylene glycol solution and stir to obtain a clear solution, then add 0.18g of NH4VO3 (99.5%, Sinopharm Group), 0.8g of silica gel (40%, Sinopharm Group) and 3g of prepared single-layer sheet structure Bi2WO6 to the above solution, and stir for 30min. After the mixed solution is dried at 80°C for 12h, the powder is placed in a porcelain boat and transferred to a muffle furnace, and calcined at 600°C in air.
[0055] Example 4
[0056] This embodiment provides a bismuth tungstate-bismuth vanadate composite catalyst, and the preparation method of the catalyst is different from the preparation method in Example 1 in that: step (4) specifically disperses the powder in 70 ml of deionized water by ultrasonic treatment for 30 minutes, and reacts in a reactor at 200° C. for 48 hours. After naturally cooling to room temperature, the product is centrifuged and washed with deionized water several times, and then the material is dried at 60° C. for 12 hours to obtain a powder, which is the catalyst.
[0057] Comparative Example 1
[0058] This comparative example provides a single-layer flaky Bi2WO6 structure, and the preparation method comprises the following steps:
[0059] First, 2mmol Bi(NO3)3·5H2O (99.0%, Sinopharm Group) was dissolved in 1M dilute nitric acid (Sinopharm Group) or ethylene glycol (99.5%, Sinopharm Group) solution and stirred to obtain a clear solution. After adding 1mmol Na2WO4·2H2O and 0.05-0.15g KBr (99.0%, Sinopharm Group), the solution was stirred evenly and then transferred into a high-pressure reactor and heated at 120°C for 24 hours to obtain a single-layer lamellar structure of Bi2WO6.
[0060] Comparative Example 2
[0061] This comparative example provides a nano-sized quantum bismuth vanadate (q-BiVO4), and the preparation method comprises the following steps:
[0062] 0.48 g of Bi(NO3)3·5H2O was dissolved in 1 M dilute nitric acid or ethylene glycol solution and stirred to obtain a clear solution, then 0.12 g of NH4VO3 (99.5%, Sinopharm Group) was added and stirred evenly, then 0.2 g of silica gel (40%, Sinopharm Group) was added and stirred evenly. After drying and calcination at 400°C, the powder was added to deionized water for ultrasonic dispersion, then transferred to a high-pressure reactor, heated at 180°C for 24 hours, centrifuged, washed, and dried at 80°C in a box oven (Model 84011, Shanghai Kanglu Instrument Equipment Co., Ltd.) to obtain q-BiVO4.
[0063] Application Example 1
[0064] This application example provides a method for catalytically synthesizing H2O2 using the bismuth tungstate-bismuth vanadate composite catalyst obtained in Example 1, comprising the following steps:
[0065] The bismuth tungstate-bismuth vanadate composite catalyst (W-0.30V) obtained in Example 1 was dispersed in a beaker filled with ethanol-water solution, and the beaker was placed in the reaction system, and then heated at 100-150 mW cm –2H2O2 was catalytically synthesized under the action of simulated solar light source (the simulated solar light source was a 500W xenon lamp BBZM-Ι type) and ultrasound (180 / 360W, 40kHz, Shenzhen Xinkaida Electronics Co., Ltd.) with a vibration frequency of 40kHz and a power of 180W; the volume ratio of ethanol to water in the ethanol-water solution was 0.20:1; the mass ratio of the catalyst to the ethanol-water solution was 0.001:1, and the temperature of the catalytic process was room temperature, which was provided by circulating cooling water.
[0066] Application Example 2
[0067] This application example provides a method for degrading RhB using the bismuth tungstate-bismuth vanadate composite catalyst obtained in Example 1, comprising the following steps:
[0068] (1) Disperse 50 mg of the bismuth tungstate-bismuth vanadate composite catalyst (W-0.30V) obtained in Example 1 into 50 ml of a 50 mg / L RhB solution, and stir for 30 minutes in a dark environment to allow the RhB solution and the catalytic material to reach an adsorption / desorption equilibrium;
[0069] (2) The solution in adsorption / desorption equilibrium in step (1) was placed under 100 mW cm -2 RhB was degraded under the action of simulated sunlight and ultrasonic vibration frequency of 40 kHz and power of 180 W. 6 ml of solution was taken at intervals of 20 minutes and the supernatant was taken. The absorbance of the clear solution at the characteristic absorption peak wavelength of RhB was tested by UV-visible spectrophotometer (Hitachi U-3310).
[0070] Comparative Application Example 1
[0071] This comparative application example provides a method for catalytically synthesizing H2O2 and degrading RhB without adding a catalyst, comprising the following steps:
[0072] The ethanol-water solution without catalyst (volume ratio of 0.20:1) and 50 ml RhB solution with a concentration of 50 mg / L were placed under ultrasound at a frequency of 40 kHz, a power of 180 W and a power of 100 mW cm -2 Under simulated sunlight irradiation and ultrasound with an ultrasonic vibration frequency of 40 kHz and a power of 180 W, the absorbance of the clarified solution at the characteristic absorption peak wavelengths of H2O2 and RhB was tested using a UV-visible spectrophotometer.
[0073] Comparative Application Example 2
[0074] This comparative application example provides a method for catalytically synthesizing H2O2 and degrading RhB without adding a catalyst, comprising the following steps:
[0075] Bi2WO6, q-BiVO4 and W-0.30V catalysts were added to ethanol-water solution (volume ratio of 0.20:1) and 50 ml RhB solution with a concentration of 50 mg / L, and then placed in 100 mW cm -2 The absorbance of the clear solution at the characteristic absorption peak wavelengths of H2O2 and RhB was tested using a UV-visible spectrophotometer under simulated sunlight.
[0076] Comparative Application Example 3
[0077] This comparative application example provides a method for catalytically synthesizing H2O2 and degrading RhB without adding a catalyst, comprising the following steps:
[0078] Bi2WO6, q-BiVO4 and W-0.30V catalysts were added to ethanol-water solution (volume ratio of 0.20:1) and 50 ml RhB solution with a concentration of 50 mg / L, and then placed in ultrasound at a frequency of 40 kHz and a power of 180 W. The absorbance of the clear solution at the characteristic absorption peak wavelengths of H2O2 and RhB was tested using a UV-visible spectrophotometer.
[0079] Comparative Application Example 4
[0080] This comparative application example provides a method for catalytically synthesizing H2O2 and degrading RhB without adding a catalyst, comprising the following steps:
[0081] Bi2WO6, q-BiVO4 and W-0.30V catalysts were added to ethanol-water solution (volume ratio of 0.20:1) and 50 ml RhB solution with a concentration of 50 mg / L, and then placed in 100 mW cm -2 Under simulated sunlight irradiation and ultrasound with an ultrasonic vibration frequency of 40 kHz and a power of 180 W, the absorbance of the clarified solution at the characteristic absorption peak wavelengths of H2O2 and RhB was tested using a UV-visible spectrophotometer.
[0082] Figure 1 (a) is a scanning electron microscope (SEM) image of Bi2WO6 in comparative example 1. It can be seen from the image that Bi2WO6 has a flaky structure and is evenly distributed.
[0083] Figure 1 (b) is the SEM image of q-BiVO4 in comparative example 2. The morphology of q-BiVO4 is a regular decahedron with nanometer size.
[0084] Figure 1 (c) is a low-resolution transmission electron microscopy (TEM) image of W-0.30V in Example 1 and Figure 1(d) is a high-resolution TEM. It can be seen from the figure that q-BiVO4 is evenly distributed on the wide and narrow surfaces of the Bi2WO6 flakes to form a heterojunction. The above figure shows that we have successfully synthesized a catalyst with a "sesame cake" structure.
[0085] Figure 2 These are the standard PDF card images of Bi2WO6 and BiVO4 and the X-ray diffraction (XRD) images of Bi2WO6, q-BiVO4 and W-0.30V. It can be seen from the figures that the diffraction peaks of the prepared Bi2WO6, q-BiVO4 and W-0.30V materials are consistent with the characteristic peaks of the standard cards of the corresponding materials, indicating that the corresponding catalyst materials have been successfully synthesized.
[0086] Figure 3 This is a comparison of the effects of catalytic synthesis of H2O2 without adding catalyst, adding Bi2WO6, q-BiVO4 and W-0.30V, and the concentration of H2O2 catalytically synthesized by Bi2WO6, q-BiVO4 and W-0.30V under light irradiation (a), ultrasound (b), light irradiation and ultrasound (c) changes with reaction time. In the same reaction time, compared with Bi2WO6 and q-BiVO4, the concentration of H2O2 synthesized by W-0.30V is the highest, indicating that the unique structure of piezoelectric materials and optical materials improves the ability to capture light and mechanical vibrations, and promotes the performance of bismuth tungstate-bismuth vanadate composite catalysts. Figure 3 (d) is a curve showing the concentration of H2O2 synthesized by W-0.30V under light, ultrasound, light and ultrasound. Under light and ultrasound, the concentration of H2O2 synthesized by W-0.30V is the highest, indicating that the unique structure of the catalyst couples the piezoelectric-optical effect, promotes the interface charge transfer of W-0.30V, and improves the performance of catalytic synthesis of H2O2.
[0087] Figure 4 This is a comparison of the effects of Bi2WO6, q-BiVO4 and W-0.30V in catalytic degradation of RhB without adding a catalyst. The curves of Bi2WO6, q-BiVO4 and W-0.30V in catalytic degradation of RhB with reaction time under light (a), ultrasound (b), light and ultrasound (c). Due to the presence of Br-, Bi2WO6 is negatively charged, which can make positively charged RhB better adsorbed on Bi2WO6, and then catalytically degrade RhB, which makes the material have more contact with RhB and improves the degradation performance of the material. It can be seen from the figure that within the same reaction time, compared with Bi2WO6 and q-BiVO4, W-0.30V has the highest degradation performance, indicating that the unique structure of piezoelectric materials and optical materials improves the ability to capture light and mechanical vibrations and promotes the degradation performance of the catalyst. Figure 4(d) is the curve of the concentration change of W-0.30V in the catalytic degradation of RhB under light, ultrasound, light and ultrasound. Under light and ultrasound, the catalytic degradation performance of W-0.30V is the best, indicating that the unique structure of the catalyst couples the piezoelectric-optical effect, promotes the charge transfer at the W-0.30V interface, produces more oxygen free radicals, and improves the performance of catalytic degradation of RhB.
[0088] Figure 5 This is a schematic diagram of the "sesame cake" structure of the bismuth tungstate-bismuth vanadate composite catalyst prepared in Example 1. It is composed of bismuth tungstate (Bi2WO6) and bismuth vanadate (BiVO4) grown thereon, the bismuth tungstate having a single-layer sheet structure, and then quantum bismuth vanadate (q-BiVO4) is grown on the single-layer sheet structure by a hydrothermal template method, and the bismuth vanadate is nanosized.
[0089] The above examples show that the present invention provides a catalyst (bismuth tungstate-bismuth vanadate composite catalyst) for synthesizing H2O2 and degrading RhB using natural light and mechanical vibration. The catalyst combines the advantages of bismuth vanadate and bismuth tungstate, constructs a unique structure of the catalyst through reasonable morphological engineering, and is easy to operate and mass produce. In addition, bismuth vanadate and bismuth tungstate are low in cost, non-toxic and recyclable. The surface of the prepared single-layer sheet structure Bi2WO6 is due to Br - The presence of makes it negatively charged, which increases the adsorption of the catalyst to the positively charged dye RhB. At the same time, it increases the contact between RhB and the catalyst, improving the degradation performance of the catalyst. The catalyst uses the coupling of piezoelectric materials and optical materials to improve the utilization rate of natural light and mechanical vibration. In particular, the sheet structure increases the contact area between the material and the reactant, increases the reaction sites, and produces more oxygen free radicals; and the ultra-thin layer reduces the transport distance of the carriers, promotes the separation of photogenerated electrons and holes, and the nano-sized quantum BiVO4 has a large specific surface area, which improves the efficiency of photon utilization.
[0090] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for preparing a bismuth tungstate-bismuth vanadate composite catalyst, characterized in that: The preparation method of the bismuth tungstate-bismuth vanadate composite catalyst comprises the following steps: S1. Preparation of monolayer bismuth tungstate by a bottom-up method assisted by KBr or hexadecyltrimethylammonium bromide; S2, growing quantum bismuth vanadate on the bismuth tungstate with a single-layer sheet structure obtained in step S1 by a hydrothermal template method to obtain the bismuth tungstate-bismuth vanadate composite catalyst; The specific process of step S1 includes the following sub-steps: S11, dissolving bismuth nitrate pentahydrate in dilute nitric acid or ethylene glycol solution and stirring to obtain a clear solution; S12, adding sodium tungstate dihydrate and KBr or sodium tungstate dihydrate and hexadecyltrimethylammonium bromide to the clear solution obtained in step S11, stirring evenly and transferring to a high-pressure reactor, reacting at 120-180° C. for 24-36 hours, and centrifuging and washing to obtain the monolayer flaky bismuth tungstate.
2. The method for preparing a bismuth tungstate-bismuth vanadate composite catalyst according to claim 1, characterized in that: The specific process of step S2 includes the following sub-steps: S21, dissolving bismuth nitrate pentahydrate in dilute nitric acid or ethylene glycol solution and stirring to obtain a clear solution; S22, adding ammonium metavanadate to the clear solution obtained in step S21, stirring evenly, adding silica gel and continuing to stir, then adding the bismuth tungstate with a single-layer sheet structure, stirring evenly, and obtaining a powder after drying and calcining; S23, adding the powder obtained in step S22 to deionized water for ultrasonic dispersion and then transferring it into a high-pressure reactor, reacting at 180-200° C. for 24-48 h, and obtaining in-situ growth of nano-sized quantum bismuth vanadate on the bismuth tungstate with the single-layer sheet structure after centrifugal washing to obtain a bismuth tungstate-bismuth vanadate composite catalyst.
3. A bismuth tungstate-bismuth vanadate composite catalyst prepared by the preparation method as described in any one of claims 1 to 2, characterized in that: The bismuth tungstate-bismuth vanadate composite catalyst comprises bismuth tungstate and bismuth vanadate grown thereon; The bismuth tungstate is a bismuth tungstate with a single-layer sheet structure, and quantum bismuth vanadate is grown on the bismuth tungstate with the single-layer sheet structure by a hydrothermal template method; the bismuth vanadate is nano-sized.
4. Use of a bismuth tungstate-bismuth vanadate composite catalyst prepared by the preparation method according to any one of claims 1 to 2 or a bismuth tungstate-bismuth vanadate composite catalyst as described in claim 3, characterized in that: The bismuth tungstate-bismuth vanadate composite catalyst is used for catalytic synthesis of H2O2.
5. The use according to claim 4, characterized in that: The specific process of using the bismuth tungstate-bismuth vanadate composite catalyst for catalytic synthesis of H2O2 comprises the following steps: S311, dispersing the bismuth tungstate-bismuth vanadate composite catalyst into an ethanol-water solution, and then –2 H2O2 is catalytically synthesized under the action of simulated solar light source and ultrasonic vibration frequency of 35-45kHz and power of 150-200 W.
6. The use according to claim 5, characterized in that: In step S311, the volume ratio of ethanol to water in the ethanol-water solution is 0.20-1:1; In step S311, the mass ratio of the bismuth tungstate-bismuth vanadate composite catalyst to the ethanol-water solution is 0.001-0.005:
1.
7. Use of a bismuth tungstate-bismuth vanadate composite catalyst prepared by the preparation method according to any one of claims 1 to 2 or a bismuth tungstate-bismuth vanadate composite catalyst as claimed in claim 3, characterized in that: The bismuth tungstate-bismuth vanadate composite catalyst is used to degrade rhodamine B.
8. The use according to claim 7, characterized in that: The specific process of using the bismuth tungstate-bismuth vanadate composite catalyst to degrade rhodamine B comprises the following steps: S321, dispersing 20-50 mg of the bismuth tungstate-bismuth vanadate composite catalyst into 50 ml of a rhodamine B solution having a concentration of 20-50 mg / L, stirring in the dark for 30-60 min, so that the rhodamine B solution and the bismuth tungstate-bismuth vanadate composite catalyst reach an adsorption-desorption equilibrium, and obtaining an adsorption-desorption equilibrium solution; S322, placing the adsorption / desorption equilibrium solution obtained in step S321 under 100-150 mW cm -2 Rhodamine B was degraded under the action of simulated sunlight and ultrasonic vibration frequency of 35-45 kHz and power of 150-200 W. 3-6 ml of the reaction clarified liquid was taken at intervals of 20-30 min and the concentration of Rhodamine B was tested by UV-visible light analyzer.