Recycling method for recovering multiple components from waste batteries
Through acid leaching and copper and aluminum removal treatment, combined with reducing agent and pH adjustment, the efficient recovery of multiple components in used batteries is achieved, which solves the problem of impurity ions affecting purity in the existing technology and realizes the recovery of high-purity products. and low-cost production.
Patent Information
- Application Number
- CN202310280632.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-21
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-03-21
Smart Images

Figure CN116443833B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of battery material recycling, and in particular relates to a recycling method for recovering multiple components from waste batteries. Background Art
[0002] As one of the electrode materials used in mainstream power batteries, lithium iron phosphate has the following characteristics: high theoretical specific capacity (170mAh / g at room temperature), stable olivine crystal structure, good thermal stability, stable voltage platform; good cycle performance, after thousands of cycles, its discharge capacity can still reach 80% of the initial capacity. Lithium-ion batteries using lithium iron phosphate still contain a high capacity of usable elements such as lithium after retirement, so this type of retired lithium-ion battery is also called "urban mine". If the elements in retired lithium-ion batteries are efficiently recycled, it can not only avoid the adverse effects of waste batteries on the environment and human health, but also achieve efficient recycling of precious metal resources.
[0003] At present, most companies only recycle lithium from lithium iron phosphate batteries, and the rest is treated as waste slag (i.e. waste phosphorus iron slag) for composting, building materials, etc. However, with the price increase of raw materials in recent years, the recycling value of this waste phosphorus iron slag is also gradually increasing. This waste phosphorus iron slag generally still contains some impurities such as aluminum oxide and copper oxide. If it is recycled by immersion in inorganic acid, these impurities will exist in the solution in the form of ions. The content of these impurities will have a great impact on the preparation of subsequent iron phosphate products, and also greatly affect the performance of the regenerated battery. Therefore, how to remove impurity ions such as aluminum and copper in the wet recovery process to improve the purity of iron phosphate is an urgent problem to be solved.
[0004] At present, the method of removing aluminum from battery powder includes resin method. For example, Chinese patent document CN113800494 A discloses a method for selectively recovering aluminum from waste lithium iron phosphate battery material acid leachate, which uses phosphonic acid-based cationic chelating resin to selectively adsorb and separate aluminum from waste lithium iron phosphate battery material acid leachate. Although this method can selectively extract aluminum, the amount of cationic chelating resin is large, and new impurity ions are introduced. The amount of acid and alkali used for adsorption and desorption is extremely large, which greatly increases the production cost and cannot be applied to industrial production. In addition, there are also organic complex precipitations for aluminum removal. For example, Chinese patent document CN113880063 A discloses a method for removing aluminum from phosphorus iron slag after lithium extraction from waste lithium iron phosphate, which selects pyridine carboxylic acid compounds, quinoline carboxylic acid compounds and isoquinoline-3-carboxylic acid compounds as aluminum removal agents. Although these organic aluminum removal agents effectively remove aluminum impurities, the aluminum removal agents cannot be recycled, and the generated organic complex precipitation can only be treated in the form of waste residues, and the economic utilization value is greatly reduced.
[0005] Therefore, there is an urgent need to find a method for better recycling waste ferrophosphorus slag in waste batteries. Summary of the invention
[0006] The purpose of the present application is to provide a method for recovering multiple components in waste batteries, aiming to solve the technical problem of how to more effectively recover waste ferrophosphorus slag in waste batteries.
[0007] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:
[0008] The present application provides a method for recovering multiple components from waste batteries, comprising:
[0009] Dismantle the used batteries and collect the waste phosphorus iron slag;
[0010] The collected waste iron-phosphorus slag is subjected to acid leaching to obtain an initial acid leaching solution containing phosphorus, iron, copper and aluminum;
[0011] Adding the initial acid leaching solution to the iron powder for copper removal treatment to obtain a copper removal acid leaching solution and a copper element product;
[0012] Adding a reducing agent to the copper removal acid leaching solution, and then adjusting the pH to 2.5-3 to perform aluminum removal treatment to obtain an aluminum removal acid leaching solution and aluminum-containing slag;
[0013] Aluminum-containing slag is acid-dissolved to obtain an aluminum-containing acid solution, the pH of the aluminum-containing acid solution is adjusted to 10-14 for precipitation reaction, and then solid-liquid separation is performed to obtain ferrous hydroxide solid slag and aluminum-containing filtrate, and the aluminum-containing filtrate is subjected to aluminum precipitation treatment to obtain an aluminum phosphate product;
[0014] The phosphorus-iron ratio of the dealuminization acid leaching solution is adjusted to be ≥1 and the pH value is 1.5-2, and an oxidant is added to perform iron precipitation treatment, and the precipitate obtained by the iron precipitation treatment is roasted to obtain an iron phosphate product;
[0015] The multiple components recovered by the recovery method include: copper element product, aluminum phosphate product and iron phosphate product.
[0016] In one embodiment, the step of subjecting the collected waste phosphorus iron slag to acid leaching to obtain an initial acid leaching solution containing phosphorus, iron, copper and aluminum includes: mixing an inorganic acid solution with the waste phosphorus iron slag at a liquid-solid ratio of 1:(4-10), then subjecting the mixture to an acid leaching reaction at 40-90° C. for 2-12 hours, and filtering to obtain carbon powder and the initial acid leaching solution.
[0017] In one embodiment, the step of adding iron powder to the initial acid leaching solution for copper removal treatment to obtain a copper-removing acid leaching solution and a copper element product includes: adding iron powder to the initial acid leaching solution at a molar ratio of 1.2 to 1.5:1 between iron powder and copper ions in the initial acid leaching solution, and then reducing the copper at 40 to 90° C. for 1 to 5 hours, and filtering to obtain a copper-removing acid leaching solution and a copper element product.
[0018] In one embodiment, the steps of adding a reducing agent to the copper removal leaching solution and adjusting the pH to 2.5-3 for aluminum removal treatment to obtain an aluminum removal acid leaching solution and aluminum-containing slag include:
[0019] According to the molar ratio of the reducing agent to the trivalent iron ion in the copper removal acid leaching solution of 1.2 to 1.5:1, the reducing agent is added to the copper removal acid leaching solution, and then an alkali reagent is added to adjust the pH of the copper removal acid leaching solution to 2.5 to 3, and the reaction is carried out at 40 to 90° C. for 1 to 5 hours, and the aluminum removal acid leaching solution and aluminum-containing slag are obtained by filtering.
[0020] In one embodiment, the reducing agent is selected from at least one of iron powder and sodium sulfite;
[0021] And / or, the alkaline agent is selected from at least one of sodium hydroxide and sodium carbonate.
[0022] In one embodiment, the step of adjusting the pH of the aluminum acid solution to 10-14 for precipitation reaction comprises:
[0023] At least one of sodium carbonate and sodium hydroxide is added to the aluminic acid solution to make the pH of the aluminic acid solution be 10 to 14, and then a precipitation reaction is carried out at 40 to 90°C.
[0024] In one embodiment, the step of subjecting the aluminum-containing filtrate to aluminum precipitation to obtain an aluminum phosphate product comprises:
[0025] The aluminum-containing filtrate is adjusted to have a phosphorus-aluminum ratio of 1:0.98-1.05 and a pH of 3.5-5.5, and then an aluminum precipitation reaction is carried out, and then the aluminum phosphate product is obtained by filtering.
[0026] In one embodiment, phosphoric acid is used to adjust the phosphorus-aluminum ratio of the aluminum-containing filtrate to 1:0.98-1.05, and sulfuric acid is used to adjust the pH of the aluminum-containing filtrate to 3.5-5.5; and / or,
[0027] The aluminum precipitation reaction includes reacting at 70 to 90° C. for 1 to 4 hours.
[0028] In one embodiment, the steps of adjusting the phosphorus-iron ratio of the dealuminization acid leaching solution to ≥1 and the pH to 1.5-2, and adding an oxidant to perform iron precipitation treatment include:
[0029] Measure the actual phosphorus-iron ratio in the dealuminization acid leaching solution, and then add trivalent iron salt or phosphorus source to adjust the phosphorus-iron ratio of the dealuminization acid leaching solution to 1-1.02:1;
[0030] An inorganic alkali solution is added to a dealuminizing acid leaching solution with a phosphorus-iron ratio of 1 to 1.02:1 to adjust the pH to 1.5 to 2, and then the oxidant is added to the dealuminizing acid leaching solution at a molar ratio of the reducing agent to the divalent iron in the dealuminizing acid leaching solution of 1 to 2:1, and the reaction is carried out at 40 to 90° C. for 3 to 5 hours; wherein the oxidant is selected from at least one of hydrogen peroxide, sodium persulfate, liquid oxygen and compressed air.
[0031] In one embodiment, the step of calcining the precipitate obtained by the iron precipitation treatment includes: calcining the precipitate at 200-800° C. for 2-12 hours.
[0032] The present application provides a method for recovering multiple components from waste batteries, mainly recovering copper single products, aluminum phosphate products and iron phosphate products from waste iron phosphate slag collected by disassembling waste batteries. Specifically, in the recovery method, the waste iron phosphate slag raw materials collected by disassembling waste batteries are subjected to acid leaching to obtain an initial acid leaching solution, and then the acid leaching solution is subjected to copper removal treatment to obtain a copper single product, and the copper removal acid leaching solution after copper removal is subjected to aluminum removal by combining with a reducing agent and pH parameters to obtain an aluminum removal acid leaching solution and aluminum-containing slag, and the aluminum-containing slag is subjected to acid dissolution, pH adjustment and aluminum precipitation treatment to obtain a high-purity aluminum phosphate product, and the aluminum removal acid leaching solution can obtain a high-purity iron phosphate product after iron precipitation treatment under certain conditions. Therefore, the above-mentioned recovery method of the present application can basically recover each multi-component in the waste iron phosphate slag in waste batteries, realize the high-efficiency recycling of elements such as copper, aluminum and iron, and the product purity is high, and there is basically no waste slag generated in the entire process, which has a good application prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0034] Figure 1 It is a schematic diagram of the process of a recycling method for recovering multiple components from waste batteries provided in an embodiment of the present application. DETAILED DESCRIPTION
[0035] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0036] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0037] In the present application, "at least one" means one or more, "more than one" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single or plural items.
[0038] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0039] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0040] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.
[0041] The terms "first", "second", and "third" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, features defined as "first", "second", and "third" may explicitly or implicitly include one or more of the features.
[0042] The embodiment of the present application provides a method for recovering multiple components from waste batteries, wherein the multiple components recovered by the method include: a copper element product, an aluminum phosphate product, and an iron phosphate product; Figure 1 As shown, the recycling method comprises the following steps:
[0043] S01: dismantle the waste batteries and collect the waste phosphorus iron slag;
[0044] S02: subjecting the collected waste phosphorus iron slag to acid leaching to obtain an initial acid leaching solution containing phosphorus, iron, copper and aluminum;
[0045] S03: adding iron powder to the initial acid leaching solution to remove copper to obtain a copper-removing acid leaching solution and a copper element product;
[0046] S04: adding a reducing agent to the copper removal acid leaching solution, and then adjusting the pH to 2.4-3 to perform aluminum removal treatment to obtain an aluminum removal acid leaching solution and aluminum-containing slag;
[0047] S05: dissolving the aluminum-containing slag with acid to obtain an aluminum-containing acid solution, adjusting the pH of the aluminum-containing acid solution to 10-14 for precipitation reaction, and then performing solid-liquid separation to obtain ferrous hydroxide solid slag and aluminum-containing filtrate, and subjecting the aluminum-containing filtrate to aluminum precipitation treatment to obtain an aluminum phosphate product;
[0048] S06: adjusting the phosphorus-iron ratio of the dealuminizing acid leaching solution to ≥1 and the pH to 1.5-2, adding an oxidant to perform iron precipitation treatment, and roasting the precipitate obtained by the iron precipitation treatment to obtain an iron phosphate product.
[0049] The embodiment of the present application provides a method for recovering multiple components from waste batteries, wherein the multiple components are mainly single copper products, aluminum phosphate products, and iron phosphate products recovered from the collected waste phosphorus iron slag. Specifically, in the recovery method, the waste phosphorus iron slag raw materials collected by disassembling the waste batteries are subjected to acid leaching to obtain an initial acid leaching solution, and then the acid leaching solution is subjected to copper removal treatment to obtain a single copper product, and the copper-removed acid leaching solution after copper removal is subjected to aluminum removal through a combination of a reducing agent and a pH parameter to obtain an aluminum-removed acid leaching solution and aluminum-containing slag, and the aluminum-containing slag is subjected to acid dissolution, pH adjustment, and aluminum precipitation treatment to obtain a high-purity aluminum phosphate product, and the aluminum-removed acid leaching solution can obtain high-purity iron phosphate dihydrate by iron precipitation treatment under certain conditions. Specifically, a reducing agent is added during the aluminum removal process to keep the iron element in the copper removal acid leaching solution in a divalent state, and the process is carried out under specific conditions of a pH of 2.5 to 3, so that trivalent aluminum is precipitated first relative to divalent iron, thereby better separating aluminum and iron. The aluminum removal acid leaching solution is subsequently treated with a phosphorus-iron ratio ≥ 1 and a pH of 1.5 to 2 to precipitate iron, thereby obtaining a high-purity iron phosphate product. The aluminum-containing slag is treated with acid dissolution, pH adjustment, and aluminum precipitation to obtain a high-purity aluminum phosphate product. In summary, the above-mentioned recovery method provided in the embodiments of the present application can recover multiple components in waste phosphorus-iron slag from waste batteries, and realize efficient recycling of elements such as copper, aluminum, and iron. There is basically no waste slag generated in the entire process, and it has a good application prospect.
[0050] For step S01: dismantle the waste batteries and collect the waste ferrophosphorus slag.
[0051] The recycling method of the embodiment of the present application has good adaptability to the waste phosphorus iron slag raw material in waste batteries. The waste phosphorus iron slag in waste batteries can be carbon-containing waste phosphorus iron slag or carbon-free waste phosphorus iron slag. Specifically, it can be the waste phosphorus iron slag remaining after the waste lithium iron phosphate positive electrode material collected and disassembled from waste lithium-ion batteries passes through the lithium element recovery process, which generally contains carbon powder and some impurities such as aluminum oxide and copper oxide.
[0052] In one embodiment, the contents of various elements in the waste ferrophosphorus slag provided by the present application are shown in Table 1.
[0053] Table 1 Main element content of waste phosphorus iron slag after lithium extraction from black powder of lithium iron phosphate waste batteries of a certain enterprise (%)
[0054] element C Fe Li Cu Al P content 38.21 24.63 0.068 0.68 0.98 14.52
[0055] For step S02: waste phosphorus iron slag collected from waste batteries is subjected to acid leaching to obtain an initial acid leaching solution containing phosphorus, iron, copper and aluminum.
[0056] The above acid leaching process of waste ferrophosphorus slag produces the following reaction equation:
[0057] FePO4+3H + =Fe 3+ +H3PO4;
[0058] Al2O3+6H + =2Al 3+ +3H2O;
[0059] CuO+2H + =Cu 2+ +H2O.
[0060] Before the acid leaching treatment, the collected waste ferrophosphorus slag may be crushed to form waste ferrophosphorus slag powder for sufficient acid leaching.
[0061] In one embodiment, an inorganic acid can be used for acid leaching. Specifically, the collected waste phosphorus iron slag is subjected to acid leaching to obtain an initial acid leaching solution containing phosphorus, iron, copper and aluminum, including: mixing the inorganic acid solution with the waste phosphorus iron slag at a liquid-solid ratio of 1: (4-10), then acid leaching for 2-12 hours at 40-90°C, and filtering to obtain carbon powder and the initial acid leaching solution. The liquid-solid ratio is in mL:g, and the inorganic acid solution is selected from at least one of hydrochloric acid solution, sulfuric acid solution and phosphoric acid solution. Taking sulfuric acid solution as an example, a 2.2-2.6 mol / L sulfuric acid solution can be selected and mixed with the waste phosphorus iron slag according to the above liquid-solid ratio for acid leaching, so that the iron, copper and aluminum in the waste phosphorus iron slag can be efficiently leached. During the acid leaching process, stirring at a stirring speed of 100 to 300 rpm / min can be used to assist in increasing the leaching rate, and the iron leaching rate is set to be 98% or more as the leaching end point. The initial acid leaching solution containing phosphorus, iron, copper, and aluminum obtained by filtration is the acid leaching solution formed at the beginning of the acid leaching process relative to the subsequent process treatment. The initial acid leaching solution is further subjected to copper removal, aluminum removal, and iron removal for recovery. The waste phosphorus iron slag can be carbon-containing waste phosphorus iron slag or carbon-free waste phosphorus iron slag. For the carbon-containing waste phosphorus iron slag, the carbon powder obtained by filtration after the acid leaching treatment can be further recovered by washing, so that the multi-products recovered by the recovery method of the embodiment of the present application also include carbon powder.
[0062] For step S03: adding the initial acid leaching solution to the iron powder to perform copper removal treatment to obtain a copper removal acid leaching solution and a copper element product.
[0063] Copper removal can return to copper elemental product. The following reaction equation occurs in this process:
[0064] Fe+Cu 2+ =Fe 2+ +Cu.
[0065] According to the content parameter of the copper ion concentration in the initial acid leaching solution after the acid leaching treatment, the amount of iron powder added is calculated so that the copper ions are recovered as copper powder precipitation, and the copper powder contains excess iron powder, which can be dissolved by the acid leaching solution or separated by magnetic separation; the copper removal acid leaching solution after the copper removal treatment is the aluminum removal acid leaching solution to be used for aluminum removal treatment. In one embodiment, the ferrous ion concentration in the copper removal acid leaching solution can be 32-35 g / l, the aluminum ion concentration can be 4.2-4.5 g / l, and the phosphorus ion concentration can be 16-20 g / l.
[0066] In one embodiment, the step of adding iron powder to the initial acid leaching solution for copper removal treatment to obtain a copper removal acid leaching solution and a copper element product includes: adding iron powder to the initial acid leaching solution according to a molar ratio of iron powder to copper ions in the initial acid leaching solution of 1.2 to 1.5:1, and then reducing copper for 1 to 5 hours at 40 to 90°C, filtering to obtain a copper removal acid leaching solution and a copper element product. The purpose of adding iron powder to the copper removal acid leaching solution is to replace and recover the copper ions in the copper removal acid leaching solution. The stoichiometric molar ratio of the amount of iron powder added to the copper ions is about 1.2 to 1.5:1, the system reaction temperature is about 40 to 90°C, and the reaction time is about 1 to 5 hours. Specifically, the copper reduction reaction can be carried out under stirring conditions of 100 to 300 r / min, and after the copper reduction reaction is completed, suction filtration is performed to separate and obtain the copper removal acid leaching solution and copper powder after copper removal. By adding iron powder to the initial acid leaching solution to achieve copper recovery, the purity of the subsequent iron phosphate product can also be improved.
[0067] For step S04: adding a reducing agent to the copper removal acid leaching solution, and then adjusting the pH to 2.5-3 to perform aluminum removal treatment to obtain an aluminum removal acid leaching solution and aluminum-containing slag.
[0068] Since ferric phosphate, ferrous phosphate and aluminum phosphate have the following parameters:
[0069] Ksp(Fe3(PO4)2)=1.0×10 -38 ,
[0070] Ksp(AlPO4·2H2O)=6.9×10 -19 ,
[0071] Ksp(FePO4·2H2O)=9.91×10 -16 ,
[0072] From the above dissolution equilibrium constant Ksp, it can be known that FePO4·2H2O precipitates after AlPO4·2H2O, and by controlling the iron concentration and pH value in the system, AlPO4·2H2O can precipitate before Fe3(PO4)2. Therefore, adding a reducing agent to the copper removal acid leaching solution can keep the iron in the copper removal acid leaching solution in the state of divalent iron, preventing the oxidation of divalent iron ions to trivalent iron ions, and the process can simultaneously adjust the pH to 2.4-3 for aluminum removal, so that trivalent aluminum precipitates before divalent iron, so as to reduce the iron loss rate during aluminum precipitation.
[0073] The above aluminum removal process produces the following reaction equation:
[0074] Al 3+ +PO4 3- +2H2O=AlPO4·2H2O
[0075] 3Fe 2+ +2PO4 3-=Fe3(PO4)2
[0076] Fe+2Fe 3+ =3Fe 2+ .
[0077] In one embodiment, the step of adding a reducing agent to the copper removal acid leaching solution and adjusting the pH to 2.5-3 for aluminum removal treatment to obtain an aluminum removal acid leaching solution and aluminum-containing slag includes: adding a reducing agent to the copper removal acid leaching solution according to a molar ratio of the reducing agent to the trivalent iron ions in the copper removal acid leaching solution of 1.2-1.5:1, then adding an alkaline reagent to adjust the pH of the copper removal acid leaching solution to 2.5-3, reacting at 40-90° C. for 1-5 hours, and filtering to obtain an aluminum acid leaching solution and aluminum-containing slag. In this way, aluminum and iron can be better separated.
[0078] Furthermore, the reducing agent can be selected from at least one of iron powder and sodium sulfite. The pH adjusting agent for adjusting the pH to 2.5 to 3 can be an alkaline agent, specifically selected from at least one of sodium hydroxide and sodium carbonate; for example, sodium carbonate powder, saturated sodium carbonate solution, sodium hydroxide, sodium hydroxide solution, and ferrous hydroxide solid slag obtained by subsequent precipitation reaction. The aluminum precipitation process can be carried out under stirring conditions of 100 to 300 r / min, so that aluminum can be better precipitated.
[0079] In the above aluminum removal process, as the precipitation is generated, the pH of the system decreases. Therefore, in order to ensure the efficiency of aluminum removal, an alkali reagent can be added in time according to the change of pH during the precipitation process of aluminum removal to maintain the pH balance, and the pH can be adjusted once every 10 to 20 minutes. Stir at the above temperature for 30 to 120 minutes, and filter to obtain aluminum-containing slag and aluminum removal acid leaching solution.
[0080] For step S05: the aluminum-containing slag is acid-dissolved to obtain an aluminum-containing acid solution, the pH of the aluminum-containing acid solution is adjusted to 10-14 for precipitation reaction, and then solid-liquid separation is performed to obtain ferrous hydroxide solid slag and aluminum-containing filtrate, and the aluminum-containing filtrate is subjected to aluminum precipitation treatment to obtain an aluminum phosphate product.
[0081] In one embodiment, the aluminum-containing slag is washed twice with water and then acid-dissolved to obtain an aluminum-containing acid solution. The step of adjusting the pH of the aluminum-containing acid solution to 10-14 for precipitation reaction comprises: adding at least one of sodium carbonate and sodium hydroxide to the aluminum-containing acid solution to make the pH of the aluminum-containing acid solution 10-14, and then performing a precipitation reaction at 40-90°C. In this process, alkali is added to adjust the pH to 10-14 to completely precipitate the ferrous ions, and the reaction is stirred under the above temperature conditions to better precipitate the ferrous ions in the aluminum-containing acid solution. The ferrous hydroxide solid slag is filtered to obtain a pH adjustment for the aluminum removal process.
[0082] In one embodiment, the step of subjecting the aluminum-containing filtrate to aluminum precipitation to obtain an aluminum phosphate product includes: adjusting the phosphorus-aluminum ratio of the aluminum-containing filtrate to 1:0.98-1.05 and the pH to 3.5-5.5, then performing an aluminum precipitation reaction, and then filtering to obtain an aluminum phosphate product. Phosphoric acid is added to the aluminum-containing filtrate to adjust the phosphorus-aluminum ratio, and the pH is continuously adjusted with dilute sulfuric acid to precipitate aluminum phosphate, and high-purity aluminum phosphate is obtained by filtration. Specifically, the phosphorus-aluminum ratio of the aluminum-containing filtrate is adjusted to 1:0.98-1.05 and the pH is adjusted to 3.5-5.5, then performing an aluminum precipitation reaction, and then filtering to obtain the aluminum phosphate product. The above-mentioned aluminum precipitation reaction process may include reacting at 70-90°C for 1-4h, so that aluminum precipitation can be better performed.
[0083] The reaction equation of aluminum slag is as follows:
[0084] AlPO4·2H2O+4OH - =AlO2 - +4H2O+PO4 3-
[0085] Fe 2+ +2OH-=Fe(OH)2
[0086] AlO2 - +PO4 3- +4H + =AlPO4·2H2O.
[0087] For step S06: the phosphorus-iron ratio of the dealuminizing acid leaching solution is adjusted to be ≥1 and the pH is 1.5-2, and an oxidant is added to perform iron precipitation treatment, and the precipitate obtained by the iron precipitation treatment is roasted to obtain an iron phosphate product.
[0088] In the above process, the phosphorus-iron ratio can be adjusted first, then the pH value can be adjusted, and finally the oxidant can be added; or the phosphorus-iron ratio can be adjusted first, then the oxidant can be added, and finally the pH value can be adjusted. There is no strict regulation on the specific order, and the ultimate goal is to ensure that the phosphorus-iron ratio of the aluminum removal acid leaching solution is ≥1, the pH is 1.5-2, and the oxidant is contained before the iron precipitation treatment. Taking hydrogen peroxide as the oxidant as an example, the reaction equation of the above iron precipitation treatment is as follows:
[0089] 2Fe 2+ +H2O2+2H + =2Fe 3+ +2H2O
[0090] Fe 3+ +PO4 3- +4H + =FePO4·2H2O.
[0091] In one embodiment, the steps of adjusting the phosphorus-iron ratio of the dealuminization acid leaching solution to ≥1 and the pH to 1.5-2, and adding an oxidant to perform iron precipitation treatment include:
[0092] The actual phosphorus-iron ratio in the dealuminating acid leaching solution is measured, and then a trivalent iron salt or a phosphorus source is added to adjust the phosphorus-iron ratio of the dealuminating acid leaching solution to 1-1.02:1; an inorganic alkali solution is added to the dealuminating acid leaching solution with a phosphorus-iron ratio of 1-1.02:1 to adjust the pH to 1.5-2, and then an oxidant is added to the dealuminating acid leaching solution according to a molar ratio of the reducing agent to the divalent iron in the dealuminating acid leaching solution of 1-2:1, and the reaction is carried out at 40-90°C for 3-5 hours; wherein the oxidant is selected from at least one of hydrogen peroxide, sodium persulfate, liquid oxygen and compressed air. Under such conditions, during the reaction process of the iron precipitation treatment, iron phosphate is precipitated and crystals grow. After the reaction is completed, the precipitate is filtered to obtain the precipitate, which is mainly high-purity dihydrate iron phosphate.
[0093] By detecting the phosphorus-iron ratio in the dealuminizing acid leaching solution, a trivalent iron salt and a phosphorus source are added according to the situation to adjust the phosphorus-iron ratio in the dealuminizing acid leaching solution to 1-1.02, and a reducing agent is added at the same time, with hydrogen peroxide as the reducing agent, and the amount of hydrogen peroxide added is about the chemical molar ratio of divalent iron ions in the solution at this time is about 1-2: 1. Then, the dealuminizing acid leaching solution is reacted under the above temperature conditions, specifically, it can be reacted under the stirring conditions of 100-300r / min for 3-5h, and finally filtered and separated to obtain dihydrate iron phosphate precipitate.
[0094] Furthermore, in the process of adjusting the phosphorus-iron ratio, the trivalent iron salt is selected from at least one of anhydrous ferric sulfate, ferric sulfate hydrate, anhydrous ferric chloride, ferric chloride hydrate and ferric nitrate; the phosphorus source is selected from at least one of phosphoric acid, ammonium dihydrogen phosphate, sodium dihydrogen phosphate, potassium dihydrogen phosphate, ammonium monohydrogen phosphate, sodium monohydrogen phosphate, sodium phosphate, potassium phosphate and ammonium phosphate. Further, the oxidant is selected from at least one of hydrogen peroxide, sodium persulfate, liquid oxygen and compressed air. The inorganic alkali solution can be ammonia water, sodium carbonate solution or sodium hydroxide solution, etc.
[0095] In one embodiment, the specific steps of roasting the precipitate obtained by the iron precipitation treatment to obtain the iron phosphate product include: the main component of the precipitate obtained by the iron precipitation treatment is dihydrate iron phosphate, and the precipitate obtained by the iron precipitation treatment is roasted at 200-800°C for 2-12h, so that an anhydrous iron phosphate product can be obtained after roasting, and after the roasting is completed, a high-purity anhydrous iron phosphate product is obtained by post-treatment (such as crushing).
[0096] In summary, the above-mentioned recovery method of multi-components from waste iron-phosphorus slag provided in the embodiment of the present application, by disassembling the waste iron-phosphorus slag raw materials collected from waste batteries for multi-component recovery, can obtain carbon powder, copper single substance products, aluminum phosphate products and iron phosphate products and other components, to achieve high purity recovery of each component. In this recovery method, the process is simple, and the introduction of other impurities can be reduced while aluminum precipitation is recovered, which greatly reduces the production cost, and the whole process is basically free of waste slag, and iron still circulates in the whole recovery process, with basically no loss. Therefore, the recovery method of the embodiment of the present application not only has less pollution, but also recovers high economic value, and is suitable for industrial large-scale production.
[0097] The following describes the invention in conjunction with specific embodiments.
[0098] Example 1
[0099] The recycling method for recovering multiple components from waste batteries is as follows
[0100] 101. Acid leaching experiment: 1000 g of carbon-containing waste phosphorus iron slag collected from waste batteries (waste phosphorus iron slag remaining after lithium recovery process of waste lithium iron phosphate positive electrode materials collected from dismantled waste lithium-ion batteries, the content of each element is shown in Table 1 above) and 2.5 mol / l of sulfuric acid are mixed at a solid-liquid ratio of 1:4, and then stirred at 300 rpm / min at 80°C for 12 h. The leaching end point is taken as the iron ion leaching rate of more than 98%. After the acid leaching is completed, the initial acid leaching solution and carbon powder are obtained by filtration. The carbon powder is further washed to obtain 388.7 g of recovered carbon powder, and the C content in the carbon powder is 98.3%.
[0101] 102. Copper removal experiment: Take 1000 ml of initial acid leaching solution (copper ion concentration 4.8 g / l), add 5.1 g of reduced iron powder, stir at room temperature (25-30°C) for 2 hours, and the stirring rate is 150 rpm / min. Excess iron powder dissolves in the acid leaching solution. After the reaction is completed, the copper ions are recovered in the form of copper elemental products. The copper recovery rate is 99.8% and the purity is 98.2%. The obtained copper removal acid leaching solution contains: ferrous ion concentration 34.2 g / l, aluminum ion concentration 4.3 g / l, phosphorus ion concentration 18.6 g / l, and copper ion concentration less than 0.01 g / l.
[0102] 103. Aluminum removal experiment: Take 988 ml of copper removal acid leaching solution after copper removal, add 7.3 g of reduced iron powder, stir at room temperature, and stir at a rate of 200 rpm / min, then add sodium hydroxide solution, adjust the pH to 2.5, heat to 70°C and stir for reaction. As the reaction proceeds, the pH drops, and the pH is adjusted once every 15 minutes, and the total stirring time is 120 minutes. After the reaction is completed, the aluminum slag and the aluminum removal acid leaching solution after aluminum removal are obtained by filtration, with an aluminum removal rate of 94.5% and an iron loss rate of 4.8%.
[0103] 104. Aluminum slag recovery experiment: 23g of aluminum slag was washed with water, 92ml of dilute sulfuric acid was added to dissolve it, and then sodium hydroxide solution was added to adjust the pH to 11, and stirred at 80℃ for 60min at a stirring rate of 300rpm / min to completely precipitate the ferrous ions. After complete precipitation, solid ferrous hydroxide slag and aluminum filtrate were obtained by filtration. The solid ferrous hydroxide slag can be used to adjust the pH of aluminum phosphate, and phosphoric acid was added to the aluminum filtrate to adjust the phosphorus-aluminum ratio to 1:1.02, and the pH was adjusted to 3.5 with dilute sulfuric acid, and stirred at 80℃ for 60min at a stirring rate of 150rpm / min. Finally, 18.1g of aluminum phosphate product was obtained by filtration, with an aluminum recovery rate of 96.2% and a purity of 98.4%.
[0104] 105. Iron phosphate precipitation experiment: Take 972 ml of the dealuminized acid leaching solution after dealuminization, add 19.5 g of 85% phosphoric acid to adjust the iron-phosphorus ratio to 1:1.02, adjust the pH to 1.5 with alkali solution, add 22.49 g of 50% hydrogen peroxide, stir at room temperature for 30 minutes, and stir at a rate of 300 rpm / min. Then heat to 80°C and stir for 3 hours to obtain dihydrate iron phosphate precipitation, crystal growth, and finally filter and roast to obtain 89.8 g of iron phosphate product, with an iron-phosphorus ratio of 0.98, a purity of 98.4%, and a total iron recovery rate of 96.6%.
[0105] The recycling method of this embodiment recovers carbon powder, copper element product, aluminum phosphate product, and iron phosphate product.
[0106] Example 2
[0107] The recycling method for recovering multiple components from waste batteries is as follows
[0108] 201. Acid leaching experiment: 1000 g of carbon-containing waste phosphorus iron slag collected from waste batteries (waste phosphorus iron slag remaining after lithium recovery process of waste lithium iron phosphate positive electrode materials collected from waste lithium-ion batteries, the content of each element is shown in Table 1 above) and 2.5 mol / l of sulfuric acid are mixed at a solid-liquid ratio of 1:4, and then stirred at 300 rpm / min at 80°C for 12 h; the leaching end point is taken as the iron ion leaching rate of more than 98%. After the acid leaching is completed, the initial acid leaching solution and carbon powder are obtained by filtration, and the carbon powder is further washed to obtain 388.7 g of recovered carbon powder, and the C content in the carbon powder is 98.3%.
[0109] 202. Copper removal experiment: Take 1000 ml of initial acid leaching solution (copper ion concentration 4.8 g / l), add 5.1 g of reduced iron powder, stir at room temperature (25-30°C) for 2 hours, and the stirring rate is 150 rpm / min. Excess iron powder is dissolved in the acid leaching solution. After the reaction is completed, the copper ions are recovered in the form of copper elemental products. The copper recovery rate is 99.8% and the purity is 98.2%. The obtained copper removal acid leaching solution contains: ferrous ion concentration 34.2 g / l, aluminum ion concentration 4.3 g / l, phosphorus ion concentration 18.6 g / l, and copper ion concentration less than 0.01 g / l.
[0110] 203. Aluminum removal experiment: Take 988 ml of copper removal acid leaching solution after copper removal, add 7.3 g of reduced iron powder, stir at room temperature, stirring at a rate of 200 rpm / min, then add sodium hydroxide solution, adjust the pH to 3.0, heat to 70°C and stir for reaction. As the reaction proceeds, the pH drops, and the pH is adjusted back every 15 minutes, and the total stirring time is 120 minutes. After the reaction is completed, the aluminum slag and the aluminum removal acid leaching solution after aluminum removal are obtained by filtration, with an aluminum removal rate of 98.4% and an iron loss rate of 10.8%.
[0111] 204. Aluminum slag recovery experiment: 29.1g aluminum slag was rinsed with water, 116ml dilute sulfuric acid was added to dissolve, and then sodium hydroxide solution was added to adjust the pH to 14, and stirred at 80℃ for 60min, with a stirring rate of 300rpm / min, to completely precipitate the ferrous ions. After complete precipitation, ferrous hydroxide solid slag and aluminum-containing filtrate were obtained by filtration. The ferrous hydroxide solid slag can be used to adjust the pH of aluminum phosphate, and phosphoric acid was added to the aluminum-containing filtrate to adjust the phosphorus-aluminum ratio to 1:1.02, and the pH was adjusted to 5.5 with dilute sulfuric acid, stirred at 80℃ for 60min, with a stirring rate of 150rpm / min, and finally 18.8g aluminum phosphate product was obtained by filtration, with an aluminum recovery rate of 98% and a purity of 99.2%.
[0112] 205, Iron phosphate precipitation experiment: Take 956ml of the dealuminized acid leaching solution after aluminum removal, add 19.2g of 85% phosphoric acid to adjust the iron-phosphorus ratio to 1:1.02, adjust the pH to 2 with alkali solution, add 22.5g of 50% hydrogen peroxide, stir at room temperature for 30min, and stir at a rate of 300rpm / min. Then heat to 80℃ and stir for 3h to obtain iron phosphate dihydrate precipitation, crystal growth, and finally filter and roast to obtain 87.7g of iron phosphate product, iron-phosphorus ratio of 1.01, purity of 99.3%, and total iron recovery rate of 96.6%.
[0113] The recycling method of this embodiment recovers carbon powder, copper element product, aluminum phosphate product, and iron phosphate product.
[0114] Example 3
[0115] The recycling method for recovering multiple components from waste batteries is as follows
[0116] 301. Acid leaching experiment: 1000 g of carbon-containing waste phosphorus iron slag collected from waste batteries (waste phosphorus iron slag remaining after lithium recovery process of waste lithium iron phosphate positive electrode materials collected from waste lithium-ion batteries, the content of each element is shown in Table 1 above) and 2.5 mol / l of sulfuric acid are mixed at a solid-liquid ratio of 1:4, and then stirred at 300 rpm / min at 80°C for 12 h; the leaching end point is taken as the iron ion leaching rate of more than 98%. After the acid leaching is completed, the initial acid leaching solution and carbon powder are obtained by filtration, and the carbon powder is further washed to obtain 388.7 g of recovered carbon powder, and the C content in the carbon powder is 98.3%.
[0117] 302. Copper removal experiment: Copper removal experiment: Take 1000 ml of initial acid leaching solution (copper ion concentration 4.8 g / l), add 5.1 g of reduced iron powder, stir at room temperature (25-30°C) for 2 hours, and the stirring rate is 150 rpm / min. Excess iron powder is dissolved in the acid leaching solution. After the reaction is completed, the copper ions are recovered in the form of copper elemental products. The copper recovery rate is 99.8% and the purity is 98.2%. The obtained copper removal acid leaching solution contains: ferrous ion concentration 34.2 g / l, aluminum ion concentration 4.3 g / l, phosphorus ion concentration 18.6 g / l, and copper ion concentration less than 0.01 g / l.
[0118] 303, aluminum removal experiment: Take 988ml of copper removal acid leaching solution after copper removal, add 7g of reduced iron powder, stir at room temperature, stirring at a rate of 200rpm / min, then add sodium hydroxide solution, adjust the pH to 3.0, heat to 70℃ and stir for reaction. As the reaction proceeds, the pH drops, and it is adjusted back once every 15min, and stirred for a total of 120min. After the reaction is completed, the aluminum slag and the aluminum removal acid leaching solution after aluminum removal are obtained by filtration, with an aluminum removal rate of 98.4% and an iron loss rate of 10.8%.
[0119] 304, aluminum slag recovery experiment: 29.1g aluminum slag was rinsed with water, 116ml dilute sulfuric acid was added to dissolve, and then sodium hydroxide solution was added to adjust the pH to 14, and stirred at 80℃ for 60min, with a stirring rate of 300rpm / min, to completely precipitate the ferrous ions. After complete precipitation, ferrous hydroxide solid slag and aluminum filtrate were obtained by filtration, and the ferrous hydroxide solid slag can be used to adjust the pH of aluminum phosphate, and phosphoric acid was added to the aluminum filtrate to adjust the phosphorus-aluminum ratio to 1:1.05, and the pH was adjusted to 5.5 with dilute sulfuric acid, and stirred at 80℃ for 60min, with a stirring rate of 150rpm / min, and finally 18.8g aluminum phosphate product was obtained by filtration, with an aluminum recovery rate of 98% and a purity of 99.2%.
[0120] 305, Iron phosphate precipitation experiment: Take 956ml of the dealuminized acid leaching solution after dealuminization, add 19.2g of 85% phosphoric acid to adjust the iron-phosphorus ratio to 1:1.0, adjust the pH to 2 with alkali solution, add 42.5g of liquid oxygen, stir at room temperature for 30min, and the stirring rate is 300rpm / min. Then heat to 80℃ and stir for 3h to obtain dihydrate iron phosphate precipitation, crystal growth, and finally filter and roast to obtain 85.7g of iron phosphate product, with an iron-phosphorus ratio of 0.98, a purity of 99.5%, and a total iron recovery rate of 95.4%.
[0121] Comparative Example 1
[0122] The aluminum removal experimental process of step 103 of Example 1 is changed to resin aluminum removal, and the steps are as follows
[0123] Acid leaching experiment: 1000g of carbon-containing waste phosphorus iron slag collected from waste batteries (waste phosphorus iron slag remaining after lithium recovery process of waste lithium iron phosphate positive electrode materials collected from waste lithium-ion batteries, the content of each element is shown in Table 1 above) and 2.5mol / l of sulfuric acid were mixed at a solid-liquid ratio of 1:4, and then stirred at 300rpm / min at 80°C for 12h; the leaching end point was taken as the iron ion leaching rate of more than 98%, and the initial acid leaching solution and carbon powder were obtained by filtration after the acid leaching was completed. The carbon powder was further washed to obtain 388.7g of recovered carbon powder, and the C content in the carbon powder was 98.3%.
[0124] Copper removal experiment: Copper removal experiment: Take 1000ml of initial acid leaching solution (copper ion concentration 4.8g / l), add 5.1g of reduced iron powder, stir at room temperature (25-30°C) for 2h, and the stirring rate is 150rpm / min. Excess iron powder dissolves in the acid leaching solution. After the reaction is completed, the copper ions are recovered in the form of copper elemental products. The copper recovery rate is 99.8% and the purity is 98.2%. The obtained copper removal solution contains: ferrous ion concentration 34.2g / l, aluminum ion concentration 4.3g / l, phosphorus ion concentration 18.6g / l, and copper ion concentration less than 0.01g / l.
[0125] Resin aluminum removal: Take 988ml of copper removal acid leaching solution and add sodium hydroxide solution to adjust the pH to 2.8. Select an ion exchange column with a diameter of 48.2mm and a length of 280mm, fill it with carboxylic acid cation chelating resin transformed by concentrated ammonia water, and use a peristaltic pump to pass the leaching solution from bottom to top through the ion exchange column at 1.0mL / min. The outflowing liquid is the aluminum removal acid leaching solution. The concentration of each metal ion is detected by ICP, and the aluminum removal rate is 88.6% and the iron loss rate is 23.3%.
[0126] Iron phosphate precipitation experiment: Take about 874 ml of the aluminum-removed acid leaching solution after aluminum removal, add 14.4 g of 85% phosphoric acid to adjust the iron-phosphorus ratio to 1:1.02, adjust the pH to 1.5 with alkali solution, add 16.9 g of 50% hydrogen peroxide, stir at room temperature for 30 minutes, and the stirring rate is 300 rpm / min. Then heat to 80 ° C and stir for 3 hours to obtain iron phosphate dihydrate precipitation, crystal growth, and finally filter and roast to obtain 74.1 g of iron phosphate product, iron-phosphorus ratio 0.88, purity 86.4%, and total iron recovery rate 72.4%.
[0127] Comparative Example 2
[0128] The aluminum removal experimental process of step 103 of Example 1 is changed to organic complex aluminum removal, and the steps are as follows
[0129] Acid leaching experiment: 1000g of carbon-containing waste phosphorus iron slag collected from waste batteries (waste phosphorus iron slag remaining after lithium recovery process of waste lithium iron phosphate positive electrode materials collected from waste lithium-ion batteries, the content of each element is shown in Table 1 above) and 2.5mol / l of sulfuric acid were mixed at a solid-liquid ratio of 1:4, and then stirred at 300rpm / min at 80°C for 12h; the leaching end point was taken as the iron ion leaching rate of more than 98%, and the initial acid leaching solution and carbon powder were obtained by filtration after the acid leaching was completed. The carbon powder was further washed to obtain 388.7g of recovered carbon powder, and the C content in the carbon powder was 98.3%.
[0130] Copper removal experiment: Copper removal experiment: Take 1000ml of initial acid leaching solution (copper ion concentration 4.8g / l), add 5.1g of reduced iron powder, stir at room temperature (25-30°C) for 2h, and the stirring rate is 150rpm / min. Excess iron powder dissolves in the acid leaching solution. After the reaction is completed, the copper ions are recovered in the form of copper elemental products. The copper recovery rate is 99.8% and the purity is 98.2%. The obtained copper removal acid leaching solution contains: ferrous ion concentration 34.2g / l, aluminum ion concentration 4.3g / l, phosphorus ion concentration 18.6g / l, and copper ion concentration less than 0.005g / l.
[0131] Organic complex aluminum removal: Take 988 ml of the copper removal acid leaching liquid after copper removal, add 59.3 g of 2-pyridinecarboxylic acid, stir at 80°C, and the stirring rate is 200 rpm / min. After filtering, 2-pyridinecarboxylic acid aluminum waste residue and filtrate, i.e., aluminum removal acid leaching liquid, are obtained. The concentration of each metal ion is detected by ICP, and the aluminum removal rate is 96.8%, and the iron loss rate is 12.6%.
[0132] Iron phosphate precipitation experiment: Take about 928ml of the aluminum-removed acid leaching solution after aluminum removal, add 17.2g of 85% phosphoric acid to adjust the iron-phosphorus ratio to 1:1.02, adjust the pH to 1.5 with alkali solution, add 20.1g of 50% hydrogen peroxide, stir at room temperature for 30min, and stir at a rate of 300rpm / min. Then heat to 80℃ and stir for 3h to obtain dihydrate iron phosphate precipitation, crystal growth, and finally filter and roast to obtain 80g iron phosphate product, iron-phosphorus ratio 0.92, purity 93.4%, and total iron recovery rate 83%.
[0133] The recovery data of the above examples and comparative examples are shown in Table 2 below.
[0134] Table 2
[0135]
[0136] As can be seen from Table 2 above, since the acid leaching and copper removal processes are the same, the copper element parameters obtained are the same. However, compared with the resin aluminum removal of Comparative Example 1 and the organic complex aluminum removal of Comparative Example 2, the embodiment of the present application adds an iron powder reducing agent to the copper removal acid leaching solution and adjusts the pH to 2.5-3 during the aluminum removal process to remove aluminum, which has a higher aluminum removal rate and a lower iron loss rate, so that the entire recovery method of the embodiment of the present application can recover more aluminum phosphate products and iron phosphate products, and the purity is high. At the same time, in the embodiment of the present application, when removing aluminum, within the range of pH 2.5-3, the higher the pH value, the higher the aluminum removal rate, and the purer the iron phosphate product obtained, and the higher the pH value when the aluminum-containing slag is recovered, the higher the aluminum recovery rate, and the purer the aluminum phosphate product. When precipitating iron phosphate, the phosphorus ratio in the iron-phosphorus ratio is increased, and hydrogen peroxide is used as an oxidant, and the final iron recovery rate is high.
[0137] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for recovering multiple components from waste batteries, characterized in that: include: Dismantle the used batteries and collect the waste phosphorus iron slag; The collected waste iron-phosphorus slag is subjected to acid leaching to obtain an initial acid leaching solution containing phosphorus, iron, copper and aluminum; Adding iron powder to the initial acid leaching solution to perform copper removal treatment to obtain a copper-removed acid leaching solution and a copper element product; According to the molar ratio of the reducing agent to the trivalent iron ions in the copper removal acid leaching solution being 1.2 to 1.5:1, the reducing agent is added to the copper removal acid leaching solution, and then the pH is adjusted to 2.5 to 3 for aluminum removal treatment to obtain an aluminum removal acid leaching solution and aluminum-containing slag; The aluminum-containing slag is acid-dissolved to obtain an aluminum-containing acid solution, the pH of the aluminum-containing acid solution is adjusted to 10-14 for precipitation reaction, and then solid-liquid separation is performed to obtain ferrous hydroxide solid slag and aluminum-containing filtrate, and the aluminum-containing filtrate is subjected to aluminum precipitation treatment to obtain an aluminum phosphate product; The phosphorus-iron ratio of the dealuminization acid leaching solution is adjusted to be ≥1 and the pH is 1.5-2, and an oxidant is added to perform iron precipitation treatment, and the precipitate obtained by the iron precipitation treatment is roasted to obtain an iron phosphate product; The multiple components recovered by the recovery method include: the copper element product, the aluminum phosphate product and the iron phosphate product.
2. The recycling method according to claim 1, characterized in that: The step of subjecting the collected waste phosphorus iron slag to acid leaching to obtain an initial acid leaching solution containing phosphorus, iron, copper and aluminum includes: mixing an inorganic acid solution with the waste phosphorus iron slag at a liquid-to-solid ratio of 1:(4-10), then subjecting the mixture to an acid leaching reaction at 40-90° C. for 2-12 hours, and filtering to obtain carbon powder and the initial acid leaching solution.
3. The recycling method according to claim 1, characterized in that: The step of adding iron powder to the initial acid leaching solution for copper removal treatment to obtain a copper-removing acid leaching solution and a copper element product comprises: adding the iron powder to the initial acid leaching solution at a molar ratio of 1.2 to 1.5:1 to the copper ions in the initial acid leaching solution, then performing a copper reduction reaction at 40 to 90° C. for 1 to 5 hours, and filtering to obtain the copper-removing acid leaching solution and the copper element product.
4. The recycling method according to claim 1, characterized in that: The steps of adding a reducing agent to the copper removal acid leaching solution and adjusting the pH to 2.5 to 3 to perform aluminum removal treatment to obtain the aluminum removal acid leaching solution and aluminum-containing slag include: The reducing agent is added to the copper removal acid leaching solution, and then an alkali agent is added to adjust the pH of the copper removal acid leaching solution to 2.5-3, reacting at 40-90° C. for 1-5 hours, and filtering to obtain the aluminum acid leaching solution and the aluminum-containing slag.
5. The recycling method according to claim 4, characterized in that: The reducing agent is selected from at least one of iron powder and sodium sulfite; And / or, the alkaline agent is selected from at least one of sodium hydroxide and sodium carbonate.
6. The recycling method according to any one of claims 1 to 5, characterized in that: The step of adjusting the pH of the aluminum acid solution to 10-14 for precipitation reaction comprises: At least one of sodium carbonate and sodium hydroxide is added to the aluminic acid solution to make the pH of the aluminic acid solution be 10 to 14, and then the precipitation reaction is carried out at 40 to 90° C.
7. The recycling method according to any one of claims 1 to 5, characterized in that: The step of subjecting the aluminum-containing filtrate to aluminum precipitation to obtain an aluminum phosphate product comprises: The aluminum-containing filtrate is adjusted to have a phosphorus-aluminum ratio of 1:0.98-1.05 and a pH of 3.5-5.5, and then an aluminum precipitation reaction is carried out, and then the aluminum phosphate product is obtained by filtering.
8. The recycling method according to claim 7, characterized in that: The phosphorus-aluminum ratio of the aluminum-containing filtrate is adjusted to 1:0.98-1.05 with phosphoric acid, and the pH of the aluminum-containing filtrate is adjusted to 3.5-5.5 with sulfuric acid; and / or, The aluminum precipitation reaction includes reacting at 70 to 90° C. for 1 to 4 hours.
9. The recycling method according to any one of claims 1 to 5, characterized in that: The steps of adjusting the phosphorus-iron ratio of the dealuminization acid leaching solution to be ≥1 and the pH to be 1.5-2, and adding an oxidant to perform iron precipitation treatment include: Measuring the actual phosphorus-iron ratio in the dealuminization acid leaching solution, and then adding a trivalent iron salt or a phosphorus source to adjust the phosphorus-iron ratio of the dealuminization acid leaching solution to 1 to 1.02:1; An inorganic alkali solution is added to the dealuminizing acid leaching solution with a phosphorus-iron ratio of 1 to 1.02:1 to adjust the pH to 1.5 to 2, and then the oxidant is added to the dealuminizing acid leaching solution at a molar ratio of the reducing agent to the divalent iron in the dealuminizing acid leaching solution of 1 to 2:1, and the reaction is carried out at 40 to 90° C. for 3 to 5 hours; wherein the oxidant is selected from at least one of hydrogen peroxide, sodium persulfate, liquid oxygen and compressed air.
10. The recycling method according to any one of claims 1 to 5, characterized in that: The step of calcining the precipitate obtained by the iron precipitation treatment comprises: calcining the precipitate at 200 to 800° C. for 2 to 12 hours.
Citation Information
Patent Citations
Method for selectively recovering aluminum from acid leaching solution of waste lithium iron phosphate battery material
CN113800494A
Method for removing aluminum from ferrophosphorus slag after lithium extraction of waste lithium iron phosphate and preparation method of battery-grade iron phosphate
CN113880063A
Method for recovering iron phosphate from iron-phosphorus slag after lithium extraction of lithium iron phosphate battery
CN111646447A
Lithium iron phosphate battery waste recycling method
CN115259126A