A water-based, curing-free, self-cleaning porcelain plate coating
By adjusting the ratio of raw materials and using the hybridization of water-based polysiloxane and hydroxyl emulsion and the cross-linking of curing agents, the stability and curing problems of porcelain plate coatings were solved, and water-based self-curing spraying with high adhesion was realized. Cleaning porcelain plate coatings improves the industrial application of porcelain coatings.
Patent Information
- Application Number
- CN202310446007.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-04-24
AI Technical Summary
Existing porcelain plate coatings have problems such as poor stability, long curing time, high temperature baking, and the coating is prone to chipping and falling off, which limits its industrial promotion.
By adjusting the ratio of raw materials, a water-based aging-free self-cleaning porcelain plate coating is prepared, including component A and component B. Component A contains water-based polysiloxane, hydroxyl emulsion, fillers, pigments, etc., and component B is The curing agent uses water-based polysiloxane hybridized with hydroxyl emulsion and cross-linked with the curing agent to form a spatial network structure. Non-stick additives are added to improve surface cleaning performance.
The porcelain plate coating is more environmentally friendly, free of aging, and has good stability. It can be sprayed at room temperature, and the workpiece does not need to be preheated. The coating has strong adhesion and good corrosion resistance, which expands the use scope and operating efficiency of the porcelain coating.
Smart Images

Figure BDA0004195642060000051 
Figure BDA0004195642060000061 
Figure BDA0004195642060000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of porcelain plate coatings, in particular to a water-based curing-free self-cleaning porcelain plate coating. Background Art
[0002] As the subway system becomes more and more complete, the requirements for the safety of locomotive interior and station interior materials are also getting higher and higher. In some locomotives and station public areas, porcelain plates are explicitly required to replace fluorocarbon plates and other organic coating plates such as powder spray plates that release highly toxic gases under open flames. The porcelain film coating on the porcelain plate is formed by organic-inorganic hybridization, with polysiloxane-hydroxy emulsion as the main body, combined with inorganic anti-aging pigments and functional inorganic fillers, and cured at room temperature to form an organic-inorganic homogeneous coating with enamel structure and performance. Water-based curing-free self-cleaning porcelain plate coating combines the characteristics of organic and inorganic coatings. The construction property tends to be organic coatings, and the coating performance tends to be inorganic coatings. It can be used in the inner wall of rail locomotives, subway stations, airports, railway stations and other public buildings. At the same time, it also has extremely low VOC emissions, is non-flammable, smokeless and non-toxic, the coating hardness can reach 4-5H, the coating particle size is micro-nano, it is not easy to collapse and fall off after a heavy impact, and can be reworked, the surface is easy to clean, the marker is easy to erase, and it has good anti-graffiti and self-cleaning properties.
[0003] In recent years, with the increasingly stringent environmental regulations, traditional fluorocarbon plates can no longer meet market needs due to their high pollution, temperature difference resistance, softening at high temperature, easy decomposition, generation of harmful smoke, coating hardness of 1-2H, soft texture, and easy scratching. Water-based, curing-free, self-cleaning porcelain plate coatings have the advantages of high temperature resistance, wear resistance, low surface energy, non-toxicity, chemical resistance, high hardness, and self-cleaning of inorganic coatings, and also include the characteristics of easy construction and strong adhesion of organic coatings, making them more and more widely used. Conventional porcelain plate coatings mainly use inorganic sols as the main film-forming substances, deionized water or other solvents as the dispersion medium, and then supplemented with pigments, fillers, additives, etc., and are prepared by stirring, dispersing, and grinding processes. However, they have the disadvantages of poor stability, long curing time, high temperature baking, and easy collapse and shedding of the paint film after heavy impact. In addition, the viscosity of the coating is low after curing, and it is easy to sag. Generally, the substrate needs to be preheated to 40-60℃ before spraying, which limits the industrial promotion of porcelain coatings. Summary of the invention
[0004] The purpose of the present invention is to provide a water-based, curing-free, self-cleaning porcelain plate coating to solve the problems of the above-mentioned prior art. The present invention prepares a more environmentally friendly, curing-free, stable, easy to construct, non-flammable, smokeless, non-toxic, self-cleaning porcelain plate coating by adjusting the raw materials and the proportion, thereby overcoming the shortcomings of conventional porcelain coatings.
[0005] To achieve the above object, the present invention provides the following solutions:
[0006] One of the technical solutions of the present invention is: a water-based curing-free self-cleaning porcelain plate coating, the water-based curing-free self-cleaning porcelain plate coating comprising component A and component B;
[0007] The component A comprises the following raw materials in parts by weight: 30-50 parts of waterborne polysiloxane, 30-50 parts of hydroxyl emulsion, 5-10 parts of filler, 10-20 parts of pigment, 0.1-1 part of thickener, 0.1-1 part of leveling agent, 0.1-1 part of defoamer, 0.1-1 part of dispersant, 1-3 parts of non-stick additive and 0-10 parts of water;
[0008] The B component is a curing agent.
[0009] Furthermore, the mass ratio of the component A to the component B is 10:(1-2).
[0010] Furthermore, the solid content of the waterborne polysiloxane is 30-50wt.%; the hydroxyl emulsion includes one or more of acrylic resin emulsion, alkyd resin emulsion and epoxy resin emulsion; the solid content of the hydroxyl emulsion is 30-50wt.%.
[0011] The preparation method of waterborne polysiloxane is:
[0012] 30 kg of polysiloxane was poured into a 50 L glass reactor and dispersed at a speed of 400-500 r / min. Ammonia and acetic acid were used to adjust the pH value of the system to 4-5. Then, the reaction was kept at 60-70 ° C for 3 hours. After the reaction was completed, 1.5 kg of trimethylmethoxysilane (silane end-capping agent) and 0.15 kg of fumed silica were added. The viscosity of the system was adjusted to 200, the pH value was adjusted to 6.5-7.5 with ammonia water and acetic acid, and the final product was collected after being allowed to stand at 40-50°C for 48 hours.
[0013] Furthermore, the polysiloxane includes two or more of octamethylcyclotetrasiloxane, γ-glycidyloxypropyltrimethoxysilane, 3-aminopropyltriethoxysilane, methyltrimethoxysilane, methacryloxypropyltrimethoxysilane and 3-mercaptopropyltriethoxysilane.
[0014] Furthermore, the filler includes one or more of silicon micropowder, kaolin, talc, barium sulfate, calcium carbonate and alumina fiber; the thickener includes one or more of hydroxyethyl cellulose, magnesium aluminum silicate, polyacrylate, polyurea and associative polyurethane.
[0015] Furthermore, the leveling agent includes one or more of acrylates, polyurethanes and polysiloxanes.
[0016] Furthermore, the defoaming agent includes one or more of silicones, polyethers and mineral oils.
[0017] Furthermore, the dispersant includes one or more of polyacrylic acid salts (sodium potassium, ammonium), modified acrylic esters, polyethyleneimine derivatives and alkyl quaternary ammonium salts.
[0018] Furthermore, the non-stick additive includes one or more of special polysiloxanes and polyether-terminated dimethyl silicone oil; the curing agent includes one or more of toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate and isophorone diisocyanate.
[0019] The second technical solution of the present invention is a method for preparing the above-mentioned water-based curing-free self-cleaning porcelain plate coating, comprising the following steps:
[0020] The water-based polysiloxane, pigment and filler are mixed evenly according to their mass fractions and then ground, and then the remaining raw materials in component A are added, and after being evenly dispersed, component B is added and mixed evenly to obtain the water-based curing-free self-cleaning porcelain plate coating.
[0021] Furthermore, the grinding is performed until the raw material particle size is less than 20 μm; and the dispersion time is 30 minutes.
[0022] The present invention discloses the following technical effects:
[0023] (1) The water-based polysiloxane in the water-based, curing-free, self-cleaning porcelain plate coating of the present invention can be hydrolyzed with deionized water to form silanol, which can be condensed with the hydroxyl emulsion to complete the organic-inorganic hybridization process, and can be further cross-linked with the curing agent in component B to form a porcelain coating film with a spatial network structure.
[0024] (2) The present invention can increase the adhesion of the coating by hybridizing the water-based polysiloxane and the hydroxyl emulsion, and improve the shortcomings of the polysiloxane coating, such as cracking, hardness and brittleness.
[0025] (3) The present invention can achieve the advantages of easy surface cleaning, easy erasability of marker pens, anti-graffiti and good self-cleaning performance by adding a non-stick additive.
[0026] (4) The water-based, curing-free, self-cleaning porcelain plate coating of the present invention has the advantages of being curing-free and having good initial stability. After adding component B, it can be sprayed at room temperature, and the workpiece does not need preheating treatment. It can also be cured at room temperature, which is more energy-saving and environmentally friendly. The workpiece surface only needs pickling and passivation, and the coating can maintain good adhesion. It also has excellent corrosion resistance, which can effectively expand the scope of use and operating efficiency of porcelain coatings. It is a green and environmentally friendly high-performance water-based coating. DETAILED DESCRIPTION
[0027] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0028] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0029] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0030] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.
[0031] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0032] The preparation method of the water-based polysiloxane used in the following examples of the present invention is as follows:
[0033] 30 kg of polysiloxane was poured into a 50 L glass reactor and dispersed at a speed of 450 r / min. Ammonia and acetic acid were used to adjust the pH value of the system to 4. Then, the reaction was kept at 70 ° C for 3 hours. After the reaction was completed, 1.5 kg of trimethylmethoxysilane (silane capping agent) and 0.15 kg of fumed silica were added. The system viscosity was adjusted to 200, the pH value was adjusted to 6.5 with ammonia water and acetic acid, and the mixture was allowed to stand at 50° C. for 48 h before filtering to collect the final product (aqueous polysiloxane).
[0034] The polysiloxane is composed of octamethylcyclotetrasiloxane, γ-glycidyloxypropyltrimethoxysilane, 3-aminopropyltriethoxysilane, methyltrimethoxysilane, methacryloxypropyltrimethoxysilane and 3-mercaptopropyltriethoxysilane in a mass ratio of 10:4:5:4:4:4.
[0035] Example 1
[0036] A water-based, curing-free, self-cleaning porcelain plate coating:
[0037] (1) The water-based, curing-free, self-cleaning ceramic plate coating is composed of component A and component B in a mass ratio of 10:1;
[0038] Table 1A Components
[0039]
[0040]
[0041] Component B is Covestro’s water-based curing agent Desmodur E 14.
[0042] (2) Preparation method: Mix water-based polysiloxane, filler and pigment, grind and filter to obtain a pigment slurry with a particle size of less than 20 μm, then add the remaining raw materials in component A and mix and stir evenly. After dispersing for 30 minutes, add component B and mix evenly to obtain a water-based, non-aging, self-cleaning porcelain plate coating.
[0043] Example 2
[0044] A water-based, curing-free, self-cleaning porcelain plate coating:
[0045] (1) The water-based, curing-free, self-cleaning ceramic tile coating is composed of component A and component B in a mass ratio of 10:2;
[0046] Table 2 Component A
[0047] Serial number Components Mass fraction Remark 1 Waterborne polysiloxane 43 Solid content: 40% 2 SSZ-172 water-based alkyd emulsion 27 Solid content: 47% 3 Calcium carbonate 7 filler 4 Copper Chrome Black 12 pigment 5 Hydroxyethyl Cellulose 0.4 Thickener 6 Rohm and Haas dispersant OROTAN 1124 0.4 Dispersants 7 SN4043 0.6 Leveling agent 8 BASF Foamaster MO NDW 0.4 Defoaming agent 9 Water-based non-stick additive P-7116 1.6 Non-stick additives 10 Deionized water 6.6 water ∑ 99
[0048] Component B is Desmodur VL 50 from Covestro.
[0049] (2) Preparation method: Mix water-based polysiloxane, filler and pigment, grind and filter to obtain a pigment slurry with a particle size of less than 20 μm, then add the remaining raw materials in component A and mix and stir evenly. After dispersing for 30 minutes, add component B and mix evenly to obtain a water-based, non-aging, self-cleaning porcelain plate coating.
[0050] Example 3
[0051] A water-based, curing-free, self-cleaning porcelain plate coating:
[0052] (1) The water-based, curing-free, self-cleaning ceramic tile coating is composed of component A and component B in a mass ratio of 10:1.3;
[0053] Table 3 Component A
[0054] Serial number Components Mass fraction Remark 1 Waterborne polysiloxane 40 Solid content: 40% 2 STW703A Water-based epoxy emulsion 25 Solid content: 52% 3 Alumina Fiber 12 filler 4 Bismuth yellow 12 pigment 5 Arkema Coapur BR-100P 0.4 Thickener 6 Lubrizol D540 Dispersant 0.6 Dispersants 7 BYK347 0.8 Leveling agent 8 BYK016 0.6 Defoaming agent 9 Water-based non-stick additive P-7116 1.6 Non-stick additives 10 Deionized water 6 water ∑ 99
[0055] Component B is Covestro XP2655.
[0056] (2) Preparation method: Mix water-based polysiloxane, filler and pigment, grind and filter to obtain a pigment slurry with a particle size of less than 20 μm, then add the remaining raw materials in component A and mix and stir evenly. After dispersing for 30 minutes, add component B and mix evenly to obtain a water-based, non-aging, self-cleaning porcelain plate coating.
[0057] Example 4
[0058] A water-based, curing-free, self-cleaning porcelain plate coating:
[0059] (1) The water-based, curing-free, self-cleaning ceramic plate coating is composed of component A and component B in a mass ratio of 10:1;
[0060] Table 4 Component A
[0061]
[0062]
[0063] Component B is Uahard 310 from United Cure Chemicals.
[0064] (2) Preparation method: Mix water-based polysiloxane, filler and pigment, grind and filter to obtain a pigment slurry with a particle size of less than 20 μm, then add the remaining raw materials in component A and mix and stir evenly. After dispersing for 30 minutes, add component B and mix evenly to obtain a water-based, non-aging, self-cleaning porcelain plate coating.
[0065] Example 5
[0066] The same as Example 1, except that the water-based curing-free self-cleaning porcelain plate coating consists of component A and component B in a mass ratio of 10:1.5; the amount of component B is 15 g.
[0067] Table 5 Component A
[0068] Serial number Components Mass fraction Remark 1 Waterborne polysiloxane 40 Solid content: 40% 2 DB3633 water-based hydroxypropyl dispersion resin 30 Solid content: 40% 3 Barium sulfate 5 filler 4 Titanium dioxide 18 pigment 5 Magnesium aluminum silicate 0.2 Thickener 6 BYK109 0.2 Dispersants 7 TEGO Glide 450 0.2 Leveling agent 8 BYK-028 0.2 Defoaming agent 9 SJ-5800 1 Non-stick additives 10 Deionized water 4.2 water ∑ 99
[0069] Example 6
[0070] The same as Example 1, except that the water-based curing-free self-cleaning porcelain plate coating consists of component A and component B in a mass ratio of 10:2; the amount of component B is 20 g.
[0071] Table 6 Component A
[0072]
[0073]
[0074] Example 7
[0075] A water-based, curing-free, self-cleaning porcelain plate coating:
[0076] (1) The water-based, curing-free, self-cleaning ceramic tile coating consists of component A and component B in a mass ratio of 10:1:
[0077] Table 7 Component A
[0078] Serial number Components Mass fraction Remark 1 Waterborne polysiloxane 40 Solid content: 40% 2 Water-based hydroxypropyl dispersion DB3602 25 Solid content: 52% 3 talcum powder 4 filler 4 Alumina Fiber 8 filler 5 Cobalt Green 12 pigment 6 BYK420 0.4 Thickener 7 EFKA 7702 aqueous dispersion 0.6 Dispersants 8 BYK333 0.8 Leveling agent 9 tego4100 0.8 Wetting and leveling agent 10 tego902W 0.2 Defoaming agent 11 BYK021 0.2 Defoaming agent 12 Non-stick additive 6900 1 Non-stick additives 13 Deionized water 6 water ∑ 99
[0079] B component is UAhard 310.
[0080] (2) Preparation method: The water-based polysiloxane, filler and pigment are mixed and stirred evenly, ground and filtered to obtain a pigment slurry with a particle size of less than 20 μm, and then the remaining raw materials in component A are added and mixed and stirred evenly. After dispersion for 30 minutes, component B is added and mixed evenly to obtain a water-based non-aging self-cleaning porcelain plate coating Example 8
[0081] A water-based, curing-free, self-cleaning porcelain plate coating:
[0082] (1) The water-based, curing-free, self-cleaning ceramic tile coating consists of component A and component B in a mass ratio of 10:1:
[0083] Table 8 Component A
[0084] Serial number Components Mass fraction Remark 1 Waterborne polysiloxane 32 Solid content: 40% 2 Water-based epoxy emulsion GS-730A 8 Solid content: 55% 3 Water-based hydroxypropyl dispersion DB3602 25 Solid content: 52% 4 Barium sulfate 6 filler 5 Alumina Fiber 8 filler 6 Titanium yellow 12 pigment 7 Deqian299 0.4 Thickener 8 BYK190 0.6 Dispersants 9 MOK-5409 0.2 Dispersants 10 BYK333 0.8 Leveling agent 11 tego902W 0.2 Defoaming agent 12 BYK021 0.2 Defoaming agent 13 Non-stick additive 6900 1 Non-stick additives 14 Deionized water 3.6 water ∑ 98
[0085] B Components Covestro 401-60.
[0086] (2) Preparation method: The water-based polysiloxane, filler and pigment are mixed and stirred evenly, ground and filtered to obtain a pigment slurry with a particle size of less than 20 μm, and then the remaining raw materials in component A are added and mixed evenly. After dispersion for 30 minutes, component B is added and mixed evenly to obtain a water-based, non-aging, self-cleaning porcelain plate coating.
[0087] Comparative Example 1
[0088] Same as Example 1, except that the waterborne polysiloxane is replaced with an equal mass of ethyl orthosilicate.
[0089] Table 9 Component A
[0090] Serial number Components Mass fraction Remark 1 Tetraethyl orthosilicate 40 Solid content: 40% 2 DB3633 water-based hydroxypropyl dispersion resin 30 Solid content: 40% 3 Barium sulfate 5 filler 4 Titanium dioxide 18 pigment 5 Magnesium aluminum silicate 0.2 Thickener 6 BYK109 0.2 Dispersants 7 TEGO Glide 450 0.2 Leveling agent 8 BYK-028 0.2 Defoaming agent 9 SJ-5800 1 Non-stick additives 10 Deionized water 4.2 water ∑ 99
[0091] Comparative Example 2
[0092] The same as Example 1, except that the DB3633 aqueous hydroxypropylene dispersion resin is replaced with an equal mass of Shiquanxing 6243 aqueous hydroxypropylene dispersion resin, and the amount of deionized water is adjusted to 5.2 parts.
[0093] Table 10 Component A
[0094] Serial number Components Mass fraction Remark 1 Waterborne polysiloxane 40 Solid content: 40% 2 Shiquanxing 6243 30 Solid content: 40% 3 Barium sulfate 5 filler 4 Titanium dioxide 18 pigment 5 Magnesium aluminum silicate 0.2 Thickener 6 BYK109 0.2 Dispersants 7 TEGO Glide 450 0.2 Leveling agent 8 BYK-028 0.2 Defoaming agent 9 SJ-5800 1 Non-stick additives 10 Deionized water 5.2 water ∑ 100
[0095] Comparative Example 3
[0096] The same as Example 1, except that the amounts of waterborne polysiloxane, DB3633 waterborne hydroxypropyl dispersion resin and deionized water are changed.
[0097] Table 11 Component A
[0098] Serial number Components Mass fraction Remark 1 Waterborne polysiloxane 30 Solid content: 40% 2 DB3633 water-based hydroxypropyl dispersion resin 40 Solid content: 40% 3 Barium sulfate 5 filler 4 Titanium dioxide 18 pigment 5 Magnesium aluminum silicate 0.2 Thickener 6 BYK109 0.2 Dispersants 7 TEGO Glide 450 0.2 Leveling agent 8 BYK-028 0.2 Defoaming agent 9 SJ-5800 1 Non-stick additives 10 Deionized water 5.2 water ∑ 100
[0099] Comparative Example 4
[0100] The same as comparative example 3, the only difference is that the amount of SJ-5800 non-stick additive and deionized water is changed.
[0101] Table 12 Component A
[0102]
[0103]
[0104] The performance of the water-based curing-free self-cleaning porcelain plate coatings prepared in the examples of the present invention and the comparative examples was measured, and compared with a commercially available three-component water-based porcelain coating (the main film-forming materials are silica sol and organosilane). The results are shown in Tables 13 and 14.
[0105] Table 13 Properties of coatings
[0106]
[0107] It can be seen from Table 13 that compared with commercially available porcelain coatings, the water-based curing-free self-cleaning porcelain plate coating prepared by the present invention has the advantages of curing-free, spraying at room temperature, good adhesion, reworkability, and self-cleaning.
[0108] Table 14
[0109]
[0110]
[0111] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A water-based, curing-free, self-cleaning porcelain plate coating, characterized in that: The water-based curing-free self-cleaning porcelain plate coating comprises component A and component B; The component A comprises the following raw materials in parts by weight: 40 parts of waterborne polysiloxane, 30 parts of hydroxyl emulsion, 5-10 parts of filler, 10-20 parts of pigment, 0.1-1 part of thickener, 0.1-1 part of leveling agent, 0.1-1 part of defoamer, 0.1-1 part of dispersant, 1-3 parts of non-stick additive and 0-10 parts of water; The B component is a curing agent; The mass ratio of component A to component B is 10:(1-2); The solid content of the waterborne polysiloxane is 30-50 wt. %; the solid content of the hydroxyl emulsion is 30-50 wt. %; the hydroxyl emulsion is DB3633 waterborne hydroxypropyl dispersion resin; The preparation method of the water-based polysiloxane is as follows: 30 kg of polysiloxane is dispersed at a speed of 400 to 500 r / min, ammonia water or acetic acid is used to adjust the pH value of the system to 4 to 5, and then the reaction is carried out at a temperature of 60 to 70° C. for 3 hours. After the reaction is completed, 1.5 kg of trimethylmethoxysilane and 0.15 kg of fumed silica 200 are added to adjust the viscosity of the system, ammonia water or acetic acid is used to adjust the pH value to 6.5 to 7.5, and the system is allowed to stand at a temperature of 40 to 50° C. for 48 hours and then filtered to obtain the water-based polysiloxane. The polysiloxane includes two or more of octamethylcyclotetrasiloxane, γ-glycidyloxypropyltrimethoxysilane, 3-aminopropyltriethoxysilane, methyltrimethoxysilane, methacryloxypropyltrimethoxysilane and 3-mercaptopropyltriethoxysilane.
2. The water-based, curing-free, self-cleaning porcelain plate coating according to claim 1, characterized in that: The filler includes one or more of silicon micropowder, kaolin, talc, barium sulfate, calcium carbonate and alumina fiber; the thickener includes one or more of hydroxyethyl cellulose, magnesium aluminum silicate, polyurea and associative polyurethane.
3. The water-based, curing-free, self-cleaning porcelain plate coating according to claim 1, characterized in that: The leveling agent includes one or more of acrylates, fluorocarbons and polysiloxanes.
4. The water-based, curing-free, self-cleaning porcelain plate coating according to claim 1, characterized in that: The defoaming agent includes one or more of silicone, polyether and mineral oil.
5. The water-based, curing-free, self-cleaning porcelain plate coating according to claim 1, characterized in that: The dispersant includes one or more of polyacrylic acid salts, modified acrylic esters, polyethyleneimine derivatives and alkyl quaternary ammonium salts.
6. The water-based, curing-free, self-cleaning porcelain plate coating according to claim 1, characterized in that The non-stick auxiliary agent includes one or more of special polysiloxanes and polyether-terminated dimethyl silicone oil; the curing agent includes one or more of toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate and isophorone diisocyanate.
7. A method for preparing the water-based, curing-free, self-cleaning porcelain plate coating according to any one of claims 1 to 6, characterized in that: The following steps are involved: The water-based polysiloxane, pigment and filler are mixed evenly according to their mass fractions and then ground, and then the remaining raw materials in component A are added, and after being evenly dispersed, component B is added and mixed evenly to obtain the water-based curing-free self-cleaning porcelain plate coating.
8. The preparation method according to claim 7, characterized in that: The grinding is performed until the raw material particle size is less than 20 μm; and the dispersion time is 30 minutes.
Citation Information
Patent Citations
No-curing high-performance ceramic water-based paint and preparation method thereof