A method for preparing CsPbBr3 nanosheets

By using oleylamine and tri-n-octylphosphine as surface-capping ligands in the synthesis of CsPbBr3 nanosheets, CsPbBr3 nanosheets were synthesized at room temperature by the microemulsion method, which solved the problem of easy shedding of surface-capping ligands and improved the nanometer Fluorescence quantum yield and optical properties of the chip.

CN116462225BActive Publication Date: 2024-10-11WUYI UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310482589.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-10-11
Estimated Expiration
2043-04-28

AI Technical Summary

Technical Problem

In the existing technology, CsPbBr3 nanomaterials suffer from difficulty in synthesis and stability problems, especially the easy shedding of surface-capping ligands, which results in reduced luminous efficiency and a red shift of the emission peak.

Method used

Using oleylamine and tri-n-octylphosphine as surface-capping ligands and acetone as a demulsifier, CsPbBr3 nanosheets were synthesized at room temperature through a microemulsion method. The strong binding force between tri-n-octylphosphine and the surface of the nanocrystal was used to inhibit the ligands. Desorption reduces defects.

Benefits of technology

The fluorescence quantum yield of CsPbBr3 nanosheets is increased to 87.1%, and the half-peak width is narrowed to 13.2nm. It has good optical properties and reduces the synthesis cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116462225B_ABST
    Figure CN116462225B_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of synthesis of nano-luminescent materials, and specifically discloses a method for preparing CsPbBr3 nanosheets. The preparation method comprises the following steps: pouring CsBr powder into HBr solution, dispersing by ultrasonic, and obtaining Cs precursor solution; pouring PbBr2 powder into organic solvent, dissolving by ultrasonic, injecting surface capping ligand, stirring, and obtaining PbBr2 precursor solution; the surface capping ligand comprises oleylamine and tri-n-octylphosphine; injecting PbBr2 precursor solution into stirring cyclohexane; then injecting Cs precursor solution, reacting; then injecting acetone, and obtaining a crude solution of CsPbBr3 nanosheets; centrifuging the crude solution, discarding the supernatant, and injecting into toluene, and obtaining. The CsPbBr3 nanosheets synthesized by the invention have high fluorescence quantum yield, which can reach 87.1%; narrow half-peak width, which is only 13.2nm, and have good optical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of synthesis of nano luminescent materials, and particularly relates to a preparation method of CsPbBr3 nanosheets. Background Art

[0002] All-inorganic metal halide perovskites have attracted wide attention due to their excellent optoelectronic properties such as long carrier lifetimes, high defect tolerance, tunable bandgaps, and narrow emission linewidths. Materials for achieving perovskite blue light emission generally include: CsPbCl3 quantum dots, CsPbClxBr 3-x quantum dots (0 < x < 3), but their development is limited by the problems of low luminescence efficiency and easy phase separation; low-dimensional CsPbBr3 nanomaterials (such as zero-dimensional CsPbBr3 quantum dots and one-dimensional CsPbBr3 nanocrystals) can also achieve perovskite blue light emission, but they all face the problems of difficult synthesis and stability.

[0003] Two-dimensional CsPbBr3 nanosheets have large exciton binding energies and short fluorescence lifetimes and are considered ideal perovskite blue light emission materials. The surface-capping ligands used in the synthesis process adsorb on the surface of the nanomaterials to isolate external moisture and oxygen, thereby reducing their impact on the inorganic layer structure, which is an essential step in the synthesis process of perovskite nanocrystals. However, the phenomenon of ligand detachment easily causes a decrease in the luminescence efficiency of CsPbBr3 nanosheets and a red shift of the emission peak.

[0004] Therefore, choosing a suitable surface-capping ligand plays a crucial role in synthesizing high-quality CsPbBr3 nanosheets. Summary of the Invention

[0005] The present invention aims to solve at least one of the technical problems existing in the above prior art. For this purpose, the present invention provides a preparation method of CsPbBr3 nanosheets. The preparation method uses oleylamine and trioctylphosphine as surface-capping ligands, acetone as a demulsifier, and protonates oleylamine with HBr, and synthesizes high-quality CsPbBr3 nanosheets by a microemulsion method at room temperature.

[0006] To solve the above technical problems, the first aspect of the present invention provides a preparation method of CsPbBr3 nanosheets, including the following steps:

[0007] Pour CsBr powder into an HBr solution, and after ultrasonic dispersion, obtain a Cs precursor solution;

[0008] Pour PbBr2 powder into an organic solvent, ultrasonically dissolve it, inject a surface-capping ligand, and stir to obtain a PbBr2 precursor solution; the surface-capping ligand includes oleylamine and trioctylphosphine;

[0009] The PbBr2 precursor solution is injected into the stirred cyclohexane; then the Cs precursor solution is injected to react; and then acetone is injected to obtain a crude solution of CsPbBr3 nanosheets;

[0010] The crude solution is centrifuged, the supernatant is discarded, and then injected into toluene to obtain the CsPbBr3 nanosheets.

[0011] Specifically, the present invention adopts a microemulsion method to synthesize two-dimensional perovskite nanosheets at room temperature, and uses oleylamine and tri-n-octylphosphine as surface capping ligands, acetone as a demulsifier, and HBr to protonate oleylamine to synthesize high-quality CsPbBr3 nanosheets. Among them: the surface capping ligand adopts a mixture of oleylamine and tri-n-octylphosphine. At present, in the process of synthesizing perovskite nanosheets, oleylamine and / or oleic acid are often used as surface capping ligands, but oleic acid is very easy to desorb from the surface of nanocrystals to induce defects. The present invention creatively introduces tri-n-octylphosphine and utilizes its strong binding force with the surface of nanocrystals to inhibit the atomic vibration and ligand desorption on the surface of CsPbBr3 nanosheets, reduce the generation of defects, and thus improve the synthesis quality of CsPbBr3 nanosheets.

[0012] In the preparation process of the CsPbBr3 nanosheets of the present invention, the corresponding precursor solution is first prepared: PbBr2 is dissolved in an organic solvent and a certain amount of oleylamine and tri-n-octylphosphine are added to obtain a PbBr2 precursor solution; CsBr is dissolved in HBr to obtain a Cs precursor solution; then the PbBr2 precursor solution is injected into vigorously stirred cyclohexane, and then the Cs precursor solution is injected; finally, acetone is added to induce the nucleation growth of the CsPbBr3 nanosheets.

[0013] As a further improvement of the above scheme, the volume ratio of oleylamine to tri-n-octylphosphine is (2-10):1.

[0014] Preferably, the volume ratio of oleylamine to tri-n-octylphosphine is (3-6):1.

[0015] As a further improvement of the above scheme, the concentration of the Cs precursor solution is 0.2-6 mmol / mL.

[0016] Preferably, the concentration of the Cs precursor solution is 0.5-1.5 mmol / mL.

[0017] As a further improvement of the above scheme, the concentration of the PbBr2 precursor solution is 0.1-2.5 mmol / mL.

[0018] Preferably, the concentration of the PbBr2 precursor solution is 0.2-1.0 mmol / mL.

[0019] As a further improvement of the above scheme, the volume ratio of the cyclohexane solution to the PbBr2 precursor solution is (7.5-30):1.

[0020] Preferably, the volume ratio of the cyclohexane solution to the PbBr2 precursor solution is (12-18):1.

[0021] As a further improvement of the above scheme, the usage of the Cs precursor solution and the PbBr2 precursor solution is in a molar ratio of Cs to Pb of (0.1-1.4):1.

[0022] Preferably, the usage of the Cs precursor solution and the PbBr2 precursor solution is in a molar ratio of Cs to Pb of (0.1-0.5):1.

[0023] As a further improvement of the above scheme, the volume ratio of the acetone to the cyclohexane is (0.1-0.4):1.

[0024] Preferably, the volume ratio of the acetone to the cyclohexane is (0.1-0.3):1.

[0025] Preferably, the organic solvent is selected from N,N-dimethylformamide (DMF) or dimethyl sulfoxide.

[0026] Preferably, the ultrasonic dispersion time is 20-30 minutes.

[0027] Preferably, the ultrasonic dissolution time is 20-35 minutes.

[0028] Preferably, the stirring speed is 900-1000 rpm.

[0029] Preferably, the reaction time is 30-40 seconds.

[0030] Preferably, the centrifugal speed is 9000-10000 rpm, and the centrifugal time is 2-3 minutes.

[0031] Compared with the prior art, the above technical solution of the present invention has at least the following technical effects or advantages:

[0032] (1) The present invention uses oleylamine and tri-n-octylphosphine as surface capping ligands, acetone as a demulsifier, and HBr to protonate oleylamine to synthesize CsPbBr3 nanosheets. Among them: the surface capping ligands (oleylamine and tri-n-octylphosphine) have a strong binding force with the surface of the nanocrystal, which inhibits the atomic vibration and ligand desorption on the surface of the CsPbBr3 nanosheets and reduces the generation of defects. The synthesized CsPbBr3 nanosheets have a high fluorescence quantum yield of up to 87.1%; a narrow half-peak width of only 13.2nm, and good optical properties.

[0033] (2) The present invention adopts a microemulsion method to synthesize CsPbBr3 nanosheets at room temperature, with a short reaction cycle and low synthesis cost. In addition, the prepared PbBr2 precursor can be stored for a long time without adding oleylamine and tri-n-octylphosphine surface capping ligands. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The emission and absorption spectra of the CsPbBr3 nanosheets prepared in Example 1;

[0035] Figure 2 This is a graph of the fluorescence quantum yield of the CsPbBr3 nanosheets prepared in Example 1;

[0036] Figure 3 This is a lateral transmission electron microscopy image of the CsPbBr3 nanosheet prepared in Example 1;

[0037] Figure 4 A transmission electron microscope image of the side thickness of the CsPbBr3 nanosheet prepared in Example 1;

[0038] Figure 5 The fluorescence spectra of CsPbBr3 nanosheets prepared in Example 1 and Comparative Examples 1-2. DETAILED DESCRIPTION

[0039] The present invention is described in detail below in conjunction with the examples, so that the technical personnel of the relevant technical field can understand the present invention. It is necessary to point out here that the examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. The non-essential improvements and adjustments made to the present invention by the skilled person in the relevant field according to the above invention content should still belong to the scope of protection of the present invention. At the same time, the raw materials mentioned below that are not described in detail are all commercially available products; the process steps or preparation methods not mentioned in detail are all process steps or preparation methods known to those skilled in the art.

[0040] Example 1

[0041] A method for preparing CsPbBr3 nanosheets comprises the following steps:

[0042] (1) Pour 0.5 mmol of CsBr powder into 0.5 mL of HBr solution (concentration 40%) and disperse by ultrasonic until it becomes colorless and transparent to obtain a Cs precursor solution;

[0043] (2) Pour 0.25 mmol of PbBr2 powder into 0.5 mL of DMF solution and sonicate until PbBr2 is completely dissolved; then inject 0.41 mL of oleylamine and 0.09 mL of tri-n-octylphosphine and stir continuously before use to obtain a turbid milky white PbBr2 precursor solution;

[0044] (3) Add 3 mL of cyclohexane to a transparent glass bottle and stir at 900 rpm; then quickly inject 0.2 mL of the PbBr2 precursor solution prepared in step (2) into the stirring cyclohexane solution and continue stirring for 30 seconds;

[0045] (4) 27.5 μL of the Cs precursor solution prepared in step (1) was injected into the stirring step (3) to react for 30 seconds; then 0.6 mL of acetone was injected to promote the nucleation and growth of CsPbBr3 nanosheets. The process was stirred for 90 seconds to obtain a crude solution of CsPbBr3 nanosheets;

[0046] (5) The crude solution obtained in step (4) was centrifuged at 9000 rpm for 2 minutes, the supernatant was discarded, and 2 mL of toluene was injected to obtain the CsPbBr3 nanosheet solution of this example.

[0047] Example 2

[0048] A method for preparing CsPbBr3 nanosheets comprises the following steps:

[0049] (1) Pour 0.5 mmol of CsBr powder into 0.5 mL of HBr solution (concentration 40%) and disperse by ultrasonic until it becomes colorless and transparent to obtain a Cs precursor solution;

[0050] (2) Pour 0.25 mmol of PbBr2 powder into 0.5 mL of DMF solution and sonicate until PbBr2 is completely dissolved; then inject 0.41 mL of oleylamine and 0.09 mL of tri-n-octylphosphine and stir continuously before use to obtain a turbid milky white PbBr2 precursor solution;

[0051] (3) Add 3 mL of cyclohexane to a transparent glass bottle and stir at 900 rpm; then quickly inject 0.2 mL of the PbBr2 precursor solution prepared in step (2) into the stirring cyclohexane solution and continue stirring for 30 seconds;

[0052] (4) 26 μL of the Cs precursor solution prepared in step (1) was injected into the stirring step (3) to react for 30 seconds; then 0.6 mL of acetone was injected to promote the nucleation and growth of CsPbBr3 nanosheets. The process was stirred for 90 seconds to obtain a crude solution of CsPbBr3 nanosheets;

[0053] (5) The crude solution obtained in step (4) was centrifuged at 9000 rpm for 2 minutes, the supernatant was discarded, and 2 mL of toluene was injected to obtain the CsPbBr3 nanosheet solution of this example.

[0054] Example 3

[0055] A method for preparing CsPbBr3 nanosheets comprises the following steps:

[0056] (1) Pour 0.5 mmol of CsBr powder into 0.5 mL of HBr solution (concentration 40%) and disperse by ultrasonic until it becomes colorless and transparent to obtain a Cs precursor solution;

[0057] (2) Pour 0.25 mmol of PbBr2 powder into 0.5 mL of DMF solution and sonicate until PbBr2 is completely dissolved; then inject 0.41 mL of oleylamine and 0.09 mL of tri-n-octylphosphine and stir continuously before use to obtain a turbid milky white PbBr2 precursor solution;

[0058] (3) Add 3 mL of cyclohexane to a transparent glass bottle and stir at 900 rpm; then quickly inject 0.2 mL of the PbBr2 precursor solution prepared in step (2) into the stirring cyclohexane solution and continue stirring for 30 seconds;

[0059] (4) 28 μL of the Cs precursor solution prepared in step (1) was injected into the stirring step (3) to react for 30 seconds; then 0.6 mL of acetone was injected to promote the nucleation and growth of CsPbBr3 nanosheets. The process was stirred for 90 seconds to obtain a crude solution of CsPbBr3 nanosheets;

[0060] (5) The crude solution obtained in step (4) was centrifuged at 9000 rpm for 2 minutes, the supernatant was discarded, and 2 mL of toluene was injected to obtain the CsPbBr3 nanosheet solution of this example.

[0061] Comparative Example 1

[0062] A method for preparing CsPbBr3 nanosheets comprises the following steps:

[0063] (1) Pour 0.5 mmol of CsBr powder into 0.5 mL of HBr solution (concentration 40%) and disperse by ultrasonic until it becomes colorless and transparent to obtain a Cs precursor solution;

[0064] (2) Pour 0.25 mmol of PbBr2 powder into 0.5 mL of DMF solution and sonicate until PbBr2 is completely dissolved; then inject 0.5 mL of oleylamine and stir continuously before use to obtain a turbid milky white PbBr2 precursor solution;

[0065] (3) Add 3 mL of cyclohexane to a transparent glass bottle and stir at 900 rpm; then quickly inject 0.2 mL of the PbBr2 precursor solution prepared in step (2) into the stirring cyclohexane solution and continue stirring for 30 seconds;

[0066] (4) 27.5 μL of the Cs precursor solution prepared in step (1) was injected into the stirring step (3) to react for 30 seconds; then 0.6 mL of acetone was injected to promote the nucleation and growth of CsPbBr3 nanosheets. The process was stirred for 90 seconds to obtain a crude solution of CsPbBr3 nanosheets;

[0067] (5) The crude solution obtained in step (4) was centrifuged at 9000 rpm for 2 minutes, the supernatant was discarded, and 2 mL of toluene was injected to obtain the CsPbBr3 nanosheet solution of this comparative example.

[0068] The only difference between Comparative Example 1 and Example 1 is that Comparative Example 1 uses oleylamine as the surface capping ligand.

[0069] Comparative Example 2

[0070] A method for preparing CsPbBr3 nanosheets comprises the following steps:

[0071] (1) Pour 0.5 mmol of CsBr powder into 0.5 mL of HBr solution (concentration 40%) and disperse by ultrasonic until it becomes colorless and transparent to obtain a Cs precursor solution;

[0072] (2) Pour 0.25 mmol of PbBr2 powder into 0.5 mL of DMF solution and sonicate until PbBr2 is completely dissolved; then inject 0.41 mL of oleylamine and 0.09 mL of oleic acid and stir continuously before use to obtain a turbid milky white PbBr2 precursor solution;

[0073] (3) Add 3 mL of cyclohexane to a transparent glass bottle and stir at 900 rpm; then quickly inject 0.2 mL of the PbBr2 precursor solution prepared in step (2) into the stirring cyclohexane solution and continue stirring for 30 seconds;

[0074] (4) 27.5 μL of the Cs precursor solution prepared in step (1) was injected into the stirring step (3) to react for 30 seconds; then 0.6 mL of acetone was injected to promote the nucleation and growth of CsPbBr3 nanosheets. The process was stirred for 90 seconds to obtain a crude solution of CsPbBr3 nanosheets;

[0075] (5) The crude solution obtained in step (4) was centrifuged at 9000 rpm for 2 minutes, the supernatant was discarded, and 2 mL of toluene was injected to obtain the CsPbBr3 nanosheet solution of this comparative example.

[0076] The only difference between Comparative Example 2 and Example 1 is that Comparative Example 2 uses oleylamine and oleic acid as surface capping ligands.

[0077] Performance Testing

[0078] Figure 1 The emission and absorption spectra of the CsPbBr3 nanosheets prepared in Example 1 are shown in Figure 1, where the horizontal axis Wavelength represents the wavelength, the vertical axis PL intensity represents the light excitation intensity, and Absorbance represents the absorbance. Figure 1 It can be seen that under the modification of tri-n-octylphosphine and oleylamine ligands, the sample exhibits strong exciton absorption at about 456 nm, and its emission peak is located at about 464 nm, with a corresponding full width at half maximum (FWHM) of 13.2 nm.

[0079] Figure 2 This is a graph of the fluorescence quantum yield of the CsPbBr3 nanosheets prepared in Example 1, where: the horizontal axis Wavelength represents the wavelength, the vertical axis Intensity represents the intensity, and Excitation represents the excitation. Figure 2 It can be seen that under the modification of tri-n-octylphosphine and oleylamine ligands, the fluorescence quantum yield (PLQY) of CsPbBr3 nanosheets can reach 87.1%.

[0080] Figure 3 This is a lateral transmission electron microscopy image of the CsPbBr3 nanosheets prepared in Example 1, which shows the lateral size morphology of the CsPbBr3 nanosheets modified with tri-n-octylphosphine and oleylamine ligands.

[0081] Figure 4 This is a transmission electron microscopy image of the lateral thickness of the CsPbBr3 nanosheets prepared in Example 1. The image shows that the lateral thickness of the CsPbBr3 nanosheets modified with tri-n-octylphosphine and oleylamine ligands is only about 3 nm, which is why the CsPbBr3 nanosheets can achieve blue light emission.

[0082] Figure 5The fluorescence spectra of CsPbBr3 nanosheets prepared in Example 1 and Comparative Examples 1-2 are shown in FIG. Figure 5 It can be seen that the fluorescence emission intensity of CsPbBr3 nanosheets modified with oleylamine alone (Comparative Example 1) or with oleylamine and oleic acid together (Comparative Example 2) is lower than that of CsPbBr3 nanosheets modified with oleylamine and tri-n-octylphosphine ligands (Example 1).

[0083] The performance of the CsPbBr3 nanosheets prepared in Example 2 and Example 3 is similar to that in Example 1, and will not be repeated here.

[0084] For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, without having to go through creative labor. Therefore, simple improvements made to the present invention by those skilled in the art based on the disclosure of the present invention should be within the protection scope of the present invention. The above embodiments are preferred embodiments of the present invention, and all processes similar to the present invention and equivalent changes made should belong to the protection scope of the present invention.

Claims

1. A CsPbBr 3 Preparation method of nanosheets, It is characterized in that The following steps are involved: Pour CsBr powder into HBr solution and disperse by ultrasonic to obtain Cs precursor solution; PbBr 2 The powder was poured into an organic solvent, dissolved by ultrasonication, and then the surface-capping ligand was injected and stirred to obtain PbBr 2 Precursor solution; the surface capping ligand comprises oleylamine and tri-n-octylphosphine; the volume ratio of oleylamine and tri-n-octylphosphine is (3-6):1; The PbBr 2 The precursor solution is injected into the stirred cyclohexane; then the Cs precursor solution is injected to react; and then acetone is injected to obtain CsPbBr 3 Crude solution of nanosheets; The crude solution was centrifuged, the supernatant was discarded, and then injected into toluene to obtain the CsPbBr 3 Nanosheets; The CsPbBr 3 The fluorescence quantum yield of the nanosheets is 87.1% and the half-peak width is 13.2nm.

2. CsPbBr according to claim 1 3 Preparation method of nanosheets, It is characterized in that The concentration of the Cs precursor solution is 0.2-6 mmol / mL.

3. CsPbBr according to claim 1 3 Preparation method of nanosheets, It is characterized in that The PbBr 2 The concentration of the precursor solution is 0.1-2.5 mmol / mL.

4. CsPbBr according to claim 1 3 Preparation method of nanosheets, It is characterized in that Cyclohexane and the PbBr 2 The volume ratio of the precursor solution is (7.5-30):

1.

5. CsPbBr according to claim 1 3 Preparation method of nanosheets, It is characterized in that The Cs precursor solution and the PbBr 2 The amount of the precursor solution used is based on a molar ratio of Cs to Pb of (0.1-1.4):

1.

6. CsPbBr according to claim 1 3 Preparation method of nanosheets, It is characterized in that The volume ratio of the acetone to the cyclohexane is (0.1-0.4):

1.

7. CsPbBr according to claim 1 3 Preparation method of nanosheets, It is characterized in that The organic solvent is selected from N,N-dimethylformamide or dimethyl sulfoxide.

8. CsPbBr according to claim 1 3 Preparation method of nanosheets, It is characterized in that The ultrasonic dispersion time is 20-30 minutes; the ultrasonic dissolution time is 20-35 minutes.

9. CsPbBr according to claim 1 3 Preparation method of nanosheets, It is characterized in that The PbBr 2 The precursor solution is injected into cyclohexane which is stirred at a speed of 900-1000 rpm; the reaction time is 30-40s; the centrifugal speed is 9000-10000 rpm, and the centrifugal time is 2-3 minutes.

Citation Information

Patent Citations

  • Synthesis method of halide perovskite type nanocrystal quantum dots

    CN113684025A

  • Blue-light perovskite quantum dot thin film, electroluminescent diode and preparation method of blue-light perovskite quantum dot thin film and electroluminescent diode

    CN114864835A

  • CsPbBr3 nanosheet as well as preparation method and application thereof

    CN115536059A