A reaction-sintered silicon carbide product containing a small amount of free silicon and a production method thereof

By optimizing the silicon carbide particle grading and bonding agent formula, combined with the stirring and grouting molding process, the free silicon content in the reacted sintered silicon carbide products is reduced, the problem of poor high-temperature usage performance is solved, and the high-temperature bending resistance of the product is significantly improved Strength and service life.

CN116462511BActive Publication Date: 2024-11-22SHENYANG STARLIGHT ADVANCED CERAMICS
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310520697.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-22
Estimated Expiration
2043-05-09

AI Technical Summary

Technical Problem

The high free silicon content in existing reactive sintered silicon carbide products leads to poor high-temperature usage performance, and there are defects of limited use in high-temperature environments.

Method used

By optimizing the silicon carbide particle grading and bonding agent formula, specific carbon black particle size and dispersant are used, combined with agitation and grouting molding processes, the free silicon content is reduced, and the product density and high-temperature usage stability are improved.

Benefits of technology

The free silicon content in silicon carbide products is achieved by less than or equal to 4%, which improves the high-temperature bending strength and service life of the product, and improves the bulk density and performance at different temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116462511B_ABST
    Figure CN116462511B_ABST
Patent Text Reader

Abstract

The embodiment of the present invention discloses a reaction-sintered silicon carbide product containing a small amount of free silicon and a production method thereof. The reaction-sintered silicon carbide product comprises the following components in parts by weight: 20-30 parts of pure water, 25-35 parts of silicon carbide micropowder, 40-65 parts of silicon carbide coarse particles, 6-10 parts of carbon black, and 1.1-2.3 parts of a binder. The reaction-sintered silicon carbide obtained by the present invention has a free silicon content of less than or equal to 4%, achieving excellent high-temperature stability and improving the high-temperature use limit of the product. After testing, the bulk density of the green body is 2.38-2.48g / cm 3 , finished product volume density 3.07-3.12g / cm 3 , the flexural strength at 20℃ is about 270-300MPa, and the flexural strength at 1200℃ is about 290-330MPa. The manufacturing strength, volume density and flexural strength of the blank at different temperatures have been greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present invention relate to the technical field of fine ceramic products, and in particular to a reaction-sintered silicon carbide product containing a small amount of free silicon and a production method thereof. Background Art

[0002] Reaction-sintered silicon carbide products are a new type of fine ceramics with many excellent properties: high strength, high hardness, good corrosion resistance, thermal shock resistance, high electrical and thermal conductivity, etc. The production sites are mainly concentrated in Shandong and Henan. Silicon carbide products have a wide range of applications, mainly in ceramic kiln tools, electronics, aerospace, semiconductors, photovoltaics, etc. The main preparation method is: using α-SiC and carbon black of different particle sizes under the action of a binder, through various molding methods to make a green body, and then sintering. At high temperature, the carbon black in the green body reacts with the infiltrated silicon to form β-SiC, and combines with α-SiC to form a dense sintered body. The excess silicon exists in the pores in the form of free silicon, thereby increasing the density of the product.

[0003] At present, there are two main production methods for reaction sintered silicon carbide. One is extrusion molding. The free silicon content in silicon carbide products is about 20%, and the volume density of the green body is 2.2g / cm 3 Above, the finished product volume density is 2.90g / cm 3 The flexural strength at 20°C is about 240MPa, and the flexural strength at 1200°C is about 250MPa. Another type of slip casting, the free silicon content in the silicon carbide product is about 10%, and the bulk density of the green body is 2.3g / cm 3 Above, the finished product volume density is 3.00g / cm 3 The flexural strength at 20°C is about 250MPa, and the flexural strength at 1200°C is about 260MPa. The free silicon content in the silicon carbide products obtained by the above two molding processes is relatively high, resulting in poor high-temperature use effect and the defect of limited use in high-temperature environments. Summary of the invention

[0004] To this end, an embodiment of the present invention provides a reaction-sintered silicon carbide product containing a small amount of free silicon and a production method thereof, so as to solve the defect that the high free silicon content in the existing reaction-sintered silicon carbide products leads to poor high-temperature performance.

[0005] In order to achieve the above purpose, the embodiment of the present invention provides the following technical solutions:

[0006] According to a first aspect of an embodiment of the present invention, a reaction-sintered silicon carbide product containing a small amount of free silicon is provided, comprising the following raw materials in parts by weight: 20-30 parts of pure water, 25-35 parts of silicon carbide powder, 40-65 parts of silicon carbide coarse particles, 6-10 parts of carbon black, and 1.1-2.3 parts of a binder; wherein,

[0007] The silicon carbide powder D 10 =0-1.2μm, D 50 =1.8-2.5μm, D 90 =5-10μm;

[0008] Calculated by weight percentage, the particle size distribution of the silicon carbide coarse particles is: 0-100 mesh 0-5%, 100-140 mesh 5-20%, 140-200 mesh 32-45%, 200-325 mesh 30-50%, and above 325 mesh 2-10%.

[0009] The applicant found that the bulk density of the product is closely related to the particle gradation of the raw silicon carbide. The more reasonable the gradation between the silicon carbide particles, the greater the bulk density of the product, and thus the higher the strength and the longer the service life. The applicant found through a large number of experiments that the preferred silicon carbide micropowder and silicon carbide coarse particles have a large particle size span and a reasonable particle gradation, which is conducive to improving the comprehensive performance of silicon carbide products.

[0010] Furthermore, the binder is composed of 0.2-0.5 parts of sodium carboxymethyl cellulose, 0.3-0.8 parts of dispersant, and 0.5-1 parts of deflocculant by weight.

[0011] Carbon black is nano-scale and can react well with infiltrated silicon to generate β-SiC. When carbon black is converted into silicon carbide with larger volume and mass, the porosity decreases. When silicon is excessive, more β-SiC can be generated by increasing the amount of carbon black, thereby increasing the density of the product. At the same time, the porosity of the green body will be further reduced, which helps to reduce the content of free silicon in the reaction-sintered silicon carbide products. Studies have found that when the amount of carbon black is increased, carbon black is easy to agglomerate and has poor dispersion, and it still cannot effectively reduce the free silicon content.

[0012] Binders are used to improve the dispersion of carbon black in water, thereby increasing the amount of carbon black added and improving the overall performance of the product. Currently, the commonly used binders are sodium carboxymethyl cellulose or sodium humate, which still have poor dispersibility, resulting in poor overall performance of the product.

[0013] Through a large number of studies, the present application has found that a specific amount of sodium carboxymethyl cellulose, a dispersant and a deflocculant are added, wherein the dispersant is a humate-silicate mixture, which is used to evenly disperse nano-scale carbon black in the mud, and the above dispersant is preferably DOLAPIX SP NEU produced by German Zschimmer Chemical; the deflocculant is a phosphate-silicate, which can make the silicon carbide particles well suspended in the mud and not easy to precipitate, and the above deflocculant is preferably GLESSFIX C 91 produced by German Zschimmer Chemical. The use of the above binder is more conducive to obtaining a uniform product while increasing the amount of carbon black used, thereby making the particles more orderly arranged during the slurry absorption process, increasing the volume density of the blank, reducing the difficulty of production, and at the same time ensuring that the carbon black can fully react with silicon to generate β-SiC, thereby achieving the effect of reducing the free silicon content in the product.

[0014] Furthermore, the carbon black D 10 =0-20nm, D 50 =30-50nm, D 90 =60-150nm.

[0015] Furthermore, the conductivity of the pure water is below 5 μs / cm.

[0016] According to a second aspect of an embodiment of the present invention, there is provided a method for preparing a reaction-sintered silicon carbide product containing a small amount of free silicon as described in any one of the above items, the method comprising:

[0017] Dissolve the binder in pure water, add silicon carbide powder, stir for 30-60 minutes, add coarse silicon carbide particles, stir for 45-60 minutes, add carbon black in small amounts and multiple times, stir rapidly for 48-72 hours, and then carry out grouting molding, demolding, drying and sintering in sequence.

[0018] Furthermore, when the carbon black added last time is completely integrated into the mud, a small amount of carbon black is added, and the adding time of the carbon black is 2-3 hours; the drying temperature is 80-120°C.

[0019] Furthermore, the sintering process is as follows: under vacuum state, room temperature -800°C, heating time 3-4h; 800-1150°C, heating time 3-4h; 1150-1350°C, heating time 2-3h; simultaneously filling with inert gas, 1350-1700°C, heating time 5-8h; filling with inert gas, 1700°C, keeping warm for 2-3h; 1700-1300°C, cooling down by filling with inert gas, after 1300°C, quickly cooling down by filling with helium.

[0020] The embodiments of the present invention have the following advantages:

[0021] The present invention conducts in-depth research on the raw materials and processes of reaction-sintered silicon carbide products, and finds that silicon carbide micropowder and silicon carbide coarse particles with a specific particle size distribution and a binder are stirred and a green body is obtained through a slip injection molding process. The green body is sintered at a high temperature to obtain a reaction-sintered silicon carbide with a free silicon content of less than or equal to 4%, thereby achieving excellent high-temperature stability and improving the high-temperature use limit of the product.

[0022] After testing, the bulk density of the green body is 2.38-2.48g / cm 3 , finished product volume density 3.07-3.12g / cm 3 The flexural strength at 20℃ is 270MPa-300MPa, and the flexural strength at 1200℃ is 290MPa-330Mpa. The manufacturing strength, volume density and flexural strength of the blank at different temperatures have been greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. Obviously, the drawings in the following description are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.

[0024] Figure 1 is the particle size distribution diagram of silicon carbide powder;

[0025] Figure 2 This is the particle morphology of silicon carbide coarse particles;

[0026] Figure 3 is the XRD pattern of the reaction-sintered silicon carbide product of Example 1;

[0027] Figure 4 This is the XRD diagram of the reaction-sintered silicon carbide product of Comparative Example 1;

[0028] Figure 5 This is the XRD diagram of the reaction-sintered silicon carbide product of Comparative Example 2;

[0029] Figure 6 This is the XRD diagram of the reaction-sintered silicon carbide product of Comparative Example 3;

[0030] Figure 7 This is a scanning electron microscope image of the reaction-sintered silicon carbide product of Example 1;

[0031] Figure 8 This is a scanning electron microscope image of the reaction-sintered silicon carbide product of Comparative Example 1;

[0032] Fig. 9This is a scanning electron microscope image of the reaction-sintered silicon carbide product of Comparative Example 2;

[0033] Fig.10 This is a scanning electron microscope image of the reaction-sintered silicon carbide product of Comparative Example 3. DETAILED DESCRIPTION

[0034] The following is a description of the implementation of the present invention by specific embodiments. People familiar with the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Example 1

[0036] This embodiment provides a reaction-sintered silicon carbide product, the raw materials of which are: 27 parts of pure water, 34 parts of silicon carbide powder, 59.5 parts of silicon carbide coarse particles, 7.5 parts of carbon black, and 1.5 parts of a binder. The binder is composed of 0.4 parts of sodium carboxymethyl cellulose, 0.6 parts of DOLAPIX SPNEU (Ziqihar Chemical, Germany), and 0.5 parts of GLESSFIX C 91 (Ziqihar Chemical, Germany) by weight.

[0037] Silicon carbide powder D 10 =1.08μm, D 50 =2.29μm, D 90 =7.47μm, its production method: 3000# silicon carbide powder and 1500# silicon carbide powder are mixed in a mass ratio of 1:3, and then grinded, filtered, dried, crushed and other processes are carried out in sequence to obtain the particle size distribution diagram as shown in the figure Figure 1 shown.

[0038] The particle size distribution of coarse silicon carbide particles is: 0-100 mesh 3.0%, 100-140 mesh 14.6%, 140-200 mesh 36.5%, 200-325 mesh 43.0%, 325 mesh fine 2.9%. Its production method: 60-70# granular sand is crushed by air flow mill, graded, shaped, screened and other processes. The particle size is nearly spherical. Its morphology is as follows Figure 2 shown.

[0039] The median diameter of carbon black is D 10 =10nm, D 50 =47nm, D 90 =85nm, carbon content is 93.2%, specific surface area is 48m 2 / cm, volatile content (950℃) 0.6%, pH value 9.0, ash content 0.30%.

[0040] The method for preparing the reaction-sintered silicon carbide product comprises the following steps:

[0041] 1) Pour purified water into a clean mixing bucket and start mixing.

[0042] 2) Add the binder to the stirring bucket in step 1) and stir for 8 minutes until the binder is completely dissolved.

[0043] 3) Add silicon carbide powder to the stirring barrel in step 2) and stir for 45 minutes.

[0044] 4) Add coarse silicon carbide particles to the stirring barrel in step 3) and stir for 30 minutes.

[0045] 5) Add carbon powder to the mixing barrel in step 4) gradually. Be sure to add it slowly and in small amounts multiple times. Each time you add it, be sure to observe whether the carbon powder added last time has been integrated into the previous mud. Only add it again after it has been fully integrated. This process takes about 3 hours.

[0046] 6) After all the carbon powder has been added, stir rapidly for 48 hours before use.

[0047] 7) Select plaster molds of different shapes according to production needs for grouting molding. The grouting time varies for different products. The grouting time for products with a thickness of about 5mm is 50 minutes.

[0048] 8) Demoulding: The clay blank removed from the plaster mould needs to be pressed firmly with a tool with good straightness to avoid deformation during the drying process.

[0049] 9) Drying at 100°C.

[0050] 10) Sintering, under vacuum state, room temperature -800℃, heating time 3h; 800-1150℃, heating time 4h; 1150-1350℃, heating time 3h; filling with inert gas at the same time, 1350-1700℃, heating time 6h, filling with inert gas, 1700℃, keeping warm for 2h, 1700-1300℃, cooling down by filling with inert gas, after 1300℃, filling with helium to quickly cool down.

[0051] Example 2

[0052] This embodiment provides a reaction-sintered silicon carbide product, which differs from the embodiment 1 only in that the weight percentage of carbon black is different. The raw materials of this embodiment are: 27 parts of pure water, 34 parts of silicon carbide powder, 59.5 parts of silicon carbide coarse particles, 8 parts of carbon black, and 1.5 parts of a binder. Among them, the binder is composed of 0.4 parts of sodium carboxymethyl cellulose, 0.6 parts of DOLAPIX SPNEU (German Zschimmer & Schwarz) and 0.5 parts of GLESSFIX C 91 (German Zschimmer & Schwarz) by weight.

[0053] The preparation method of the reaction-sintered silicon carbide product of this embodiment is the same as that of Example 1.

[0054] Example 3

[0055] This embodiment provides a reaction-sintered silicon carbide product, which differs from the embodiment 1 only in that the weight percentage of carbon black is different. The raw materials of this embodiment are: 27 parts of pure water, 34 parts of silicon carbide micropowder, 59.5 parts of silicon carbide coarse particles, 12 parts of carbon black, and 1.5 parts of a binder. Among them, the binder is composed of 0.4 parts of sodium carboxymethyl cellulose, 0.6 parts of DOLAPIX SPNEU (German Zschimmer & Schwarz) and 0.5 parts of GLESSFIX C 91 (German Zschimmer & Schwarz) by weight.

[0056] The preparation method of the reaction-sintered silicon carbide product of this embodiment is the same as that of Example 1.

[0057] Comparative Example 1

[0058] This comparative example provides a reaction-sintered silicon carbide product, which differs from Example 1 only in that the silicon carbide powder and silicon carbide coarse particles used are different. The raw materials used in this comparative example are: 27 parts of pure water, silicon carbide powder F1200 (D 10 =0-2.5μm, D 50 =3.5-6.5μm, D 90 =5-9μm, Shenyang Changxin New Materials Co., Ltd.) 34 parts, silicon carbide coarse particles F240 (D 10 =10-30μm, D 50 =35-75μm, D 90 =50-80μm, Shenyang Changxin New Materials Co., Ltd.) 59.5 parts, carbon black 6.5 parts, binder 1.5 parts. Among them, the binder is composed of 0.4 parts of sodium carboxymethyl cellulose, 0.6 parts of sodium humate, and 0.5 parts of GLESSFIX162 (German Zimmermann Chemical Silicate) by weight.

[0059] The preparation method of the reaction-sintered silicon carbide product in this comparative example is the same as that in Example 1.

[0060] Comparative Example 2

[0061] This comparative example provides a reaction-sintered silicon carbide product, which differs from Example 1 only in that the binder is different. The raw materials used in this comparative example are: 27 parts of pure water, 34 parts of silicon carbide micropowder of Comparative Example 1, 59.5 parts of silicon carbide coarse particles of Comparative Example 1, 6.5 parts of carbon black, and 1.5 parts of binder. Among them, the binder is composed of 0.4 parts of sodium carboxymethyl cellulose, 0.6 parts of DOLAPIX SPNEU (German Zschimmer & Schwarz) and 0.5 parts of GLESSFIX C 91 (German Zschimmer & Schwarz) by weight.

[0062] The preparation method of the reaction-sintered silicon carbide product in this comparative example is the same as that in Example 1.

[0063] Comparative Example 3

[0064] This comparative example provides a reaction-sintered silicon carbide product, which differs from Example 1 only in that the binder is different. The raw materials used in this comparative example are: 27 parts of pure water, 34 parts of silicon carbide powder of Example 1, 59.5 parts of silicon carbide coarse particles of Example 1, 6.5 parts of carbon black, and 1.5 parts of binder. Among them, the binder is composed of 0.4 parts of sodium carboxymethyl cellulose, 0.6 parts of sodium humate, and 0.5 parts of GLESSFIX162 (German Zimmermann Chemical silicate) by weight.

[0065] The preparation method of the reaction-sintered silicon carbide product in this comparative example is the same as that in Example 1.

[0066] Test Example 1

[0067] Table 1 Comparison of various properties of the produced reaction sintered bodies

[0068] Table 1

[0069]

[0070] Although the present invention has been described in detail above by general description and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements can be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all belong to the scope of protection claimed by the present invention.

Claims

1. A reaction-sintered silicon carbide product containing a small amount of free silicon, characterized in that: The raw materials include the following parts by weight: 27 parts of pure water, 34 parts of silicon carbide powder, 59.5 parts of silicon carbide coarse particles, 12 parts of carbon black, and 1.5 parts of a binder, wherein: The silicon carbide powder D 10 =1.08μm, D 50 =2.29μm, D 90 =7.47 μm; In terms of weight percentage, the particle size distribution of the silicon carbide coarse particles is: 0-100 mesh 3.0%, 100-140 mesh 14.6%, 140-200 mesh 36.5%, 200-325 mesh 43.0%, 325 mesh and finer 2.9%; The binder is composed of 0.4 parts of sodium carboxymethyl cellulose, 0.6 parts of dispersant and 0.5 parts of decoagulant by weight; The dispersant is a humate-silicate mixture; the decoagulant is a phosphate-silicate; The carbon black D 10 =10nm, D 50 =47nm, D 90 =85nm; The production method of the reaction-sintered silicon carbide product comprises: Dissolve the binder in pure water, add silicon carbide powder, stir for 30-60 minutes, add coarse silicon carbide particles, stir for 45-60 minutes, add carbon black in small amounts and multiple times, and after adding, stir rapidly for 48-72 hours, then perform grouting molding, demoulding, drying, and sintering in sequence; When the carbon black added last time is completely integrated into the mud, add a small amount of carbon black, the adding time of the carbon black is 2-3h; the drying temperature is 80-120℃; The sintering process is as follows: under vacuum state, room temperature - 800 ° C, heating time 3-4h; 800-1150 ° C, heating time 3-4h; 1150-1350 ° C, heating time 2-3h; simultaneously filling with inert gas, 1350-1700 ° C, heating time 5-8h; filling with inert gas, 1700 ° C, heat preservation 2-3h; 1700-1300 ° C, cooling by filling with inert gas, after 1300 ° C, quickly cooling by filling with helium.

2. The reaction-sintered silicon carbide product containing a small amount of free silicon according to claim 1, characterized in that: The conductivity of the pure water is below 5 μs / cm.

Citation Information

Patent Citations

  • Preparation method of high-density low-free-silicon-content reactively-sintered silicon carbide ceramic material

    CN111574226A

  • Silicon carbide roller bar material for roller kiln and preparation method of silicon carbide roller bar material

    CN114213131A

  • High-performance low-free-silicon-content reactive sintering silicon carbide ceramic material and preparation method thereof

    CN115057707A

  • Reaction bonded silicon infiltrated silicon carbide ceramic body - has continuous silicon carbide particle size distribution allowing high packing density

    DE4243864A1