A 3D printed ceramic hollow three-dimensional coil skeleton structure and a manufacturing method thereof

Through 3D printing technology and finite element simulation optimization, combined with light-curing molding and high-temperature and high-pressure sintering, the problems of complex three-dimensional coil skeleton procedures and low yield rate in traditional processes have been solved, and high-precision, high-strength and high-temperature-resistant ceramic wisps have been achieved. Three-dimensional coil bobbin manufacturing.

CN116462514BActive Publication Date: 2024-10-01CHINA NAT PETROLEUM CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210033953.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-12
Publication Date
2024-10-01
Estimated Expiration
2042-01-12

AI Technical Summary

Technical Problem

The existing three-dimensional coil skeleton is produced through traditional processes with complex procedures, low yield, and high cost. It is difficult to meet the stability and accuracy requirements in high-temperature and high-pressure environments.

Method used

3D printing technology is used to manufacture the ceramic hollow three-dimensional coil skeleton. The structure is optimized through finite element simulation. The skeleton body is printed using light curing molding technology, and is degreased and sintered in a high-temperature and high-pressure environment to form a high-strength, low-density, high-temperature-resistant structure. Ceramic structure.

Benefits of technology

It achieves high-precision molding of parts, reduces material waste and processing costs, improves yield and stability, is suitable for high temperature and high pressure environments, and has high strength, high toughness and thermal conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116462514B_ABST
    Figure CN116462514B_ABST
Patent Text Reader

Abstract

The present invention discloses a 3D printed ceramic hollow three-dimensional coil skeleton structure and a manufacturing method thereof. The three-dimensional coil skeleton is used to produce a three-dimensional ceramic coil skeleton, which greatly broadens the design ideas, bypasses the constraints of traditional processing methods, and can adopt more diverse structural forms and external shapes, which not only ensures the performance of the parts but also reduces material waste, reduces the processing cost of parts, and improves the yield rate of parts. The three-dimensional coil skeleton parts produced by the method of the present invention have the characteristics of high strength, high toughness, high wear resistance, low density, high temperature resistance, non-magnetic, non-conductive, etc., especially in a high temperature environment. The thermal deformation is small, the thermal conductivity is high, and the stability is good. The design and manufacturing method of the present invention is used to design and manufacture the three-dimensional coil skeleton, and the parts can be accurately formed. The ceramic degreasing and sintering are carried out by high temperature and high pressure protection. The manufactured parts are formed in one time, and the manufacturing accuracy and yield rate of the parts are much higher than those of the traditional process methods.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of well detection, and in particular relates to a 3D printed ceramic hollow three-dimensional coil skeleton structure and a manufacturing method thereof. Background Art

[0002] The three-dimensional ceramic coil skeleton is a key component in the three-dimensional array induction logging instrument. It is the winding carrier of the induction coil in the instrument. The three-dimensional coil skeleton is a three-dimensional structure with three groups of mutually perpendicular conductive coils wound on the skeleton for transmitting and receiving instrument signals. The three-dimensional coil skeleton has a complex structure, irregular shape and high dimensional accuracy. The three-dimensional coil skeleton is installed inside the instrument and can be tested in oil wells more than 6,000 meters underground, withstanding high temperature and high pressure from the formation. In order to enable the instrument to work reliably in this environment, the instrument is filled with hydraulic oil and the three-dimensional coil skeleton is immersed in the hydraulic oil. Therefore, the three-dimensional coil skeleton must meet the requirements of working reliably at a high temperature of 175°C and a pressure environment of 140MPa, and it must have good stability, high strength and hardness, small deformation, no oil absorption, no magnetism, and no conductivity.

[0003] Three-dimensional coil skeletons are usually made of ceramic materials. The characteristics of ceramic materials are high strength and hardness, high brittleness, and easy cracking during production. Traditional production processes are used to produce blanks, sinter them, and finally grind them into shape. The entire processing process is complicated, with many tooling, low yield, and high costs, which seriously restricts the production of parts and large-scale application of instruments. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a 3D printed ceramic hollow three-dimensional coil skeleton structure and a manufacturing method thereof, so as to solve the problem of complex processes when the three-dimensional coil skeleton is produced by traditional processes in the prior art.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A 3D printed ceramic hollow three-dimensional coil skeleton structure, comprising a three-dimensional coil skeleton, the three-dimensional coil skeleton is a cylindrical barrel structure, and the three-dimensional coil skeleton is provided with coaxial mounting holes along its length direction;

[0007] The three-dimensional coil skeleton is a hollow skeleton structure, which includes a hollow transverse support and a hollow longitudinal support; the hollow transverse support and the hollow longitudinal support are perpendicular to each other, and the hollow transverse support and the hollow longitudinal support are both arranged on the radial surface of the three-dimensional coil skeleton;

[0008] An upper end surface support and a lower end surface support are respectively provided on the two end surfaces of the three-dimensional coil skeleton, and a ring-shaped middle support is provided on the body of the three-dimensional coil skeleton;

[0009] The upper end surface support and the lower end surface support are both provided with XY winding grooves, and the XY winding grooves on the upper end surface support are connected with the XY winding grooves on the lower end surface support;

[0010] The three-dimensional coil skeleton structure is made by sintering silicon nitride ceramic material.

[0011] A further improvement of the present invention is:

[0012] Preferably, a positioning pin hole is provided on the inner side wall of the mounting hole.

[0013] Preferably, a plurality of degreasing holes are provided in the three-dimensional coil skeleton, and the degreasing holes are arranged along the length direction of the three-dimensional coil skeleton, and two ends of the degreasing holes are respectively arranged on the upper end surface support and the lower end surface support.

[0014] Preferably, the degreasing holes are equally divided along the estimated circumference of the three-dimensional coil.

[0015] Preferably, the XY winding grooves are arranged in two groups, and each group includes two symmetrical XY winding grooves.

[0016] Preferably, the end of the XY winding groove includes a wire accommodating groove and a wire passing groove, and the wire passing groove connects the wire accommodating groove and the outer end surface of the three-dimensional coil skeleton; the width of the wire accommodating groove is greater than the width of the wire passing groove.

[0017] Preferably, the wire accommodating grooves at both ends of an XY winding groove are symmetrically arranged relative to the center point of the XY winding groove.

[0018] A method for preparing a 3D printed ceramic hollow three-dimensional coil skeleton structure comprises the following steps:

[0019] Step 1, designing a three-dimensional coil skeleton structure;

[0020] Step 2, performing stress analysis on the three-dimensional coil skeleton structure by finite element simulation technology;

[0021] Step 3, optimizing the three-dimensional coil skeleton structure through force analysis structure;

[0022] Step 4, printing a three-dimensional coil skeleton structure blank by photocuring molding technology; the powder used in the photocuring molding technology is a mixed powder composed of silicon nitride powder, curing resin powder and concentrator powder;

[0023] Step 5: Degreasing and sintering the printed three-dimensional coil skeleton structure blank to complete the preparation of the three-dimensional coil skeleton structure.

[0024] Preferably, in step 4, in the photo-stereolithography manufacturing method, a stabilizer and an inert diluent are added to the mixed powder; during the printing process of the blank, the mixed powder layer thickness is 10-20 μm.

[0025] Preferably, in step 4, the degreasing and sintering process is as follows: placing the three-dimensional coil skeleton structure blank in a heating furnace, keeping it at 600-700°C for 3-4 hours; and then keeping it at 1600-1700°C for more than 10 hours.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The present invention discloses a 3D printed ceramic hollow three-dimensional coil skeleton structure. The three-dimensional coil skeleton is used to produce three-dimensional ceramic coil skeletons, which greatly broadens the design ideas, bypasses the constraints of traditional processing methods, and can adopt more diverse structural forms and external shapes, which not only ensures the performance of the parts but also reduces material waste, reduces the processing cost of parts, and improves the yield rate of parts. The three-dimensional coil skeleton parts produced by the method of the present invention have the characteristics of high strength, high toughness, high wear resistance, low density, high temperature resistance, non-magnetic, non-conductive, etc., especially in high temperature environments. The thermal deformation is small, the thermal conductivity is high, and the stability is good. The design and manufacturing method of the present invention is used to design and manufacture the three-dimensional coil skeleton, and the parts can be accurately formed. The ceramic degreasing and sintering are carried out using a high temperature and high pressure protection method. The manufactured parts are formed in one time, and the manufacturing accuracy and yield rate of the parts are much higher than those of the traditional process methods.

[0028] The present invention also discloses a method for manufacturing a 3D printed ceramic hollow three-dimensional coil skeleton structure. This method uses a 3D printing additive manufacturing method to make the prepared parts high in precision and easy to implement. A new type of coil skeleton produced by using 3D printing technology for structural molding and then using ceramic sintering technology for final shaping eliminates the problem of ceramic materials cracking due to brittleness during processing, greatly improving part processing efficiency and yield rate. Advanced processes are used to control part production and manufacturing, improve part stability and consistency, and improve part production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 Schematic diagram of the structure of a three-dimensional coil; (a) is the main view; (b) is the side view;

[0030] Figure 2 It is a structural stereogram of a three-dimensional coil skeleton;

[0031] Figure 3 It is a cross-sectional view of the AA section of the three-dimensional coil skeleton;

[0032] Figure 4 This is the structural diagram of the XY winding slot.

[0033] in:

[0034] 1-three-dimensional coil skeleton; 2-X coil group; 3-Y coil group; 4-Z coil group; 5-positioning pin hole; 6-mounting hole; 7-upper end surface support; 8-end surface wire groove; 9-XY winding groove; 10-Z winding groove; 11-degreasing hole; 12-middle support; 13-lower end surface support; 14-hollow horizontal support; 15-hollow longitudinal support; 16-wire storage groove; 17-wire groove. DETAILED DESCRIPTION

[0035] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0036] In the description of the present invention, it should be noted that the orientations or positional relationships indicated by the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inside", "outside", etc. are based on the orientations or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention; the terms "first", "second", and "third" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance; in addition, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection or a detachable connection; it can be directly connected or indirectly connected through an intermediate medium, and it can be the internal communication of two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0037] See also Figure 1 One of the implementation cases of the present invention is to provide a 3D printed ceramic hollow three-dimensional coil skeleton. The three-dimensional coil is the core component of the three-dimensional array induction logging instrument. It is a sensor device in the instrument that transmits electromagnetic disturbance signals and receives formation response information. The three-dimensional coil is composed of Figure 1As shown, it is mainly composed of a three-dimensional coil skeleton 1, an X coil group 2, a Y coil group 3 and a Z coil group 4. Among them, the X coil group 2 and the Y coil group 3 are respectively composed of two groups of multi-turn coils symmetrically arranged in the upper and lower directions; the Z coil group 4 is composed of multi-turn coils evenly arranged in the axial direction; the three-dimensional coil skeleton 1 is made of silicon nitride ceramic material sintered as a whole, and has the characteristics of high strength, low density, high temperature resistance, non-magnetic, non-conductive, etc., especially in a high temperature environment, small thermal deformation, high thermal conductivity, and good thermal stability. The three-dimensional coil skeleton 1 is the winding carrier of the three groups of X, Y, and Z coil groups, and is also an insulator for insulating the three groups of coil groups from other components; in the three-dimensional induction logging instrument, multiple three-dimensional coils are combined and used together to form an array coil group for the identification and measurement of the three-dimensional information of the formation. The three-dimensional coil is installed in the instrument, surrounded by hydraulic oil, connected to the external pressure and temperature, and is required to be able to be used reliably for a long time under a temperature of 175°C and a pressure of 140MPa.

[0038] For details, see Figure 1 , Figure 2 and Figure 3 , including positioning pin hole 5, mounting hole 6, upper end face support 7, end face wire groove 8, XY winding groove 9, Z winding groove 10, degreasing hole 11, middle support 12, lower end face support 13, hollow transverse support 14, hollow longitudinal support 15, etc. The three-dimensional coil skeleton 1 is provided with mounting hole 6 along its length direction, and the mounting hole 6 is coaxial with the three-dimensional coil skeleton 1; the mounting hole 6 is provided with positioning pin hole 5 along its inner wall at one end, and the positioning pin hole 5 is provided along the length direction of the mounting hole 6. The positioning pin hole 5 and the mounting hole 6 are used for the installation and positioning of the three-dimensional coil in the instrument. The two groups of multi-turn coils in the X coil are symmetrical with respect to the first radial line, and the first radial line is a radial line that intersects with the axis of the mounting hole 6 and is perpendicular to the axis. The two groups of multi-turn coils in the Y coil are symmetrical with respect to the second radial line, and the second radial line is a radial line that intersects with the axis of the mounting hole 6 and is perpendicular to the axis of the mounting hole 6. The first radial line and the second radial line are perpendicular to each other.

[0039] The overall structure of the three-dimensional coil skeleton 1 is a hollow skeleton structure, and the hollow skeleton structure includes a hollow transverse support 14 and a hollow longitudinal support 15. The hollow longitudinal support 15 and the hollow transverse support 14 are perpendicular to each other and are both arranged on the radial surface of the mounting hole 6. The hollow longitudinal support 15 and the hollow transverse support are equally divided along the length direction of the mounting hole 6. The middle hollow structure can facilitate the degreasing of parts, optimize the ceramic sintering process, improve the yield rate of parts, reduce the thickness of parts at various locations, make the embryonic structure of parts more uniform, speed up the 3D printing and sintering degreasing of parts, and improve the production efficiency of parts. At the same time, a plurality of interlaced hollow transverse supports 14 and hollow longitudinal supports 15 are added to the hollow structure, which can not reduce the overall strength of the parts and provide strong support for the outer structure of the skeleton.

[0040] Specifically, along the length of the three-dimensional coil skeleton 1, the upper end surface support 7 and the lower end surface support 13 are respectively arranged at both ends of the three-dimensional coil skeleton 1, and in the middle position of the three-dimensional coil skeleton 1, an intermediate support 12 is arranged along its circumference. The upper end surface support 7, the intermediate support 12 and the lower end surface support 13 are all annular support members, and the inner circle of the upper end surface support 7 and the lower end surface support 13 has the same inner diameter as the mounting hole 6 and is coaxial, and the width of the upper end surface support 7 and the lower end surface support 13 is greater than the wall thickness of the three-dimensional coil skeleton 1; the intermediate support 12 is arranged around the outer wall of the three-dimensional coil skeleton 1. The width of the upper end surface support 7 and the lower end surface support 13 protruding from the outer wall of the three-dimensional coil skeleton 1 is equal to the width of the intermediate support 12. The upper end surface support 7, the intermediate support 12, the lower end surface support 13, and the end surface wire groove 8 are used to support and fix the X and Y coils. Four XY winding grooves 9 are arranged on the upper end surface support 7, and are arranged symmetrically in pairs. Two symmetrical XY winding grooves 9 form a group, and the two groups of XY winding grooves 9 are used to load and wind the X coil and the Y coil respectively. Each XY winding groove 9 runs through the entire three-dimensional coil skeleton 1 along the length direction of the three-dimensional coil skeleton 1. The XY winding groove 9 is a fixed groove for the X and Y coils, which can not only meet the requirements of accurate winding of the XY coils, but also ensure that the coils are fixed and do not fall out of the grooves. Each XY winding groove 9 passes through the three support surfaces of the upper end surface support 7, the middle support 12 and the lower end surface support 13.

[0041] The cross-sectional structure of each XY winding slot 9 is as follows: Figure 4 As shown: it includes two parts, a wire accommodating groove 16 and a wire passing groove 17, which are connected. The wire accommodating groove 16 is used for coil winding and fixing, and is located on the end face of the coil frame. The two wire accommodating grooves used to wind a coil are symmetrically distributed, and the groove edges of the wire accommodating groove 16 are parallel to each other, so that after the coil is wound, the coil is in a regular rectangle and evenly arranged on the frame, and at the same time, the X and Y coils are perpendicular to each other; the wire passing groove 17 is a transition hole during winding, and the wire passing groove 17 connects the wire accommodating groove 16 with the outer wall of the three-dimensional coil frame 1. In order to make the space of the wire accommodating groove 16 large enough, the width of the wire passing groove 17 should be small to meet the needs of wire passing. The setting of the wire passing groove 17 makes it difficult for the X coil and the Y coil to separate.

[0042] Several degreasing holes 11 are equally divided along the circumference of the three-dimensional coil skeleton 1, and preferably there are 4 degreasing holes 11. The two ends of each degreasing hole 11 are respectively arranged on the upper end surface support 7 and the lower end surface support 13, and each degreasing hole 11 runs through the length direction of the three-dimensional coil skeleton 1. The degreasing hole 11 is a production process hole, which is used as a precipitation channel for the solidified resin in the embryo structure to be degreasing when the coil skeleton body 1 is sintered; the hollow transverse support 14 and the hollow longitudinal support 15 are reinforcing ribs in the hollow structure to increase the strength of the parts.

[0043] The performance of the three-dimensional coil mainly depends on the accuracy and stability of the three-dimensional coil skeleton 1. The present embodiment provides a method for manufacturing a 3D printed ceramic hollow three-dimensional coil skeleton, which is specifically a method for producing the three-dimensional coil skeleton 1 by combining digital design and 3D printing technology. The advantages of this method are that it uses digital technology for structural design and optimization, uses 3D printing technology for precise molding, and uses high temperature and high pressure protection to perform ceramic degreasing and sintering. The manufactured parts are formed in one step, and the manufacturing accuracy and yield of the parts are much higher than those of traditional process methods. This method includes the following processes: 1. Model design, 2. Finite element analysis of parts, 3. Optimization of the three-dimensional coil skeleton structure, 4. 3D printing molding, 5. Degreasing and sintering molding. Among them, the three steps of model design, finite element analysis, and structural optimization are completed by professional computer software (such as: SOLIDWORK, MSC and other software). The steps of the method described in the present invention are as follows:

[0044] (1) Use computer simulation technology (SOLIDWORK software) to conduct preliminary design of the three-dimensional coil skeleton structure to meet the function and structural requirements of the parts;

[0045] (2) Use finite element simulation technology (MSC software) to perform stress analysis on the three-dimensional coil skeleton structure to find stress concentration points and redundant structures, providing a basis for structural optimization;

[0046] (3) Using digital technology, we optimize the structure according to the finite element simulation results, eliminate stress concentration points, reduce redundant structures, and topologically integrate the structure, so that the bearing capacity of the parts structure is increased, the weight is reduced, and the local thickness is reduced, forming a Figure 2 The hollow three-dimensional coil skeleton structure shown in the figure includes positioning pin holes 5, mounting holes 6, upper end surface supports 7, end surface wire grooves 8, XY winding grooves 9, Z winding grooves 10, degreasing holes 11, middle supports 12, lower end surface supports 13, hollow transverse supports 14, hollow longitudinal supports 15 and other structures, among which the XY winding grooves 9 are further divided into two parts: a wire accommodating groove 16 and a wire passing groove 17. Figure 3 As shown, this structural form makes the thickness of the part embryo more uniform and the size smaller, which is beneficial to the 3D printing and degreasing sintering of the part, and improves the part yield rate. In order not to reduce the overall strength of the part, a plurality of interlaced hollow horizontal supports 14 and hollow longitudinal supports 15 are added to the hollow structure to provide strong support for the outer structure of the skeleton.

[0047] (4) 3D printing: After the part model design is finalized, it is digitally decomposed and the printing program is compiled. In this process, the ceramic powder needs to be screened and prepared. The powder used for the three-dimensional coil skeleton 1 is a mixed powder composed of silicon nitride powder, curing resin powder, and concentrator powder. Among them, silicon nitride powder is the main raw material for ceramic molding, accounting for 60-70% by volume, curing resin powder is used as a curing agent for blank molding during 3D printing, accounting for 25-35% by volume, and concentrator powder is used to concentrate laser energy, accounting for 5% by volume to help the melting and bonding of the curing resin to form the silicon nitride powder. The rest are auxiliary ingredients such as stabilizers and inert diluents. 3D printing selects conventional light-curing molding technology (SL), uses a mechanical scraper to accurately spread powder, and the thickness of each layer of powder is controlled between 15-20μm. The laser head is controlled by digital technology, and the resin powder is solidified by a laser beam. Then, the powder is spread on the molding surface and stacked layer by layer to obtain a high-precision three-dimensional coil skeleton embryo structure. Use 3D printing technology to manufacture part prototypes, select photo-stereolithography (SL) printing technology as the printing method, select a mixed powder consisting of silicon nitride powder, curing resin powder, and concentrator powder as the printing powder, use a mechanical scraper to accurately spread the powder in layers during printing, use digital control technology to accurately move the laser head, use concentrator powder to collect laser energy, use the laser beam to melt the curing resin to solidify the silicon nitride powder, and then stack layer by layer and print in a cycle to eventually form a precise part prototype structure.

[0048] (5) Degreasing and sintering: After the three-dimensional coil skeleton 1 is printed and formed, the accuracy and size of each part basically meet the requirements of the finished product. However, in order to perform the subsequent sintering, the three-dimensional coil skeleton embryo is micro-processed and finely polished, and finally enters the high-pressure nitrogen furnace for degreasing and sintering. The degreasing is carried out in the nitrogen furnace. The embryo is heated to 600-700°C in a heating furnace filled with nitrogen for 1 hour, and kept warm at normal pressure for 3-4 hours to melt the solidified resin and slowly precipitate. The degreasing hole 11 allows the solidified resin in the hollow structure of the part to flow out quickly, reducing the cracking of the parts caused by the uneven precipitation of the curing agent. The nitrogen protects the embryo from oxidation in a high temperature environment. After the solidified resin is completely precipitated, the temperature is raised to 1600-1700°C within 0.5 hours, and the pressure in the nitrogen furnace is raised to 10MPa to fully sinter the silicon nitride powder together in the nitrogen. The heat preservation is continued for more than 10 hours to promote the growth of silicon nitride grains, and finally form a silicon nitride ceramic with uniform lattice and denseness.

[0049] The three-dimensional coil skeleton parts produced in this way have the characteristics of high strength, high toughness, high wear resistance, low density, high temperature resistance, non-magnetic, non-conductive, etc., especially in high temperature environment, small thermal deformation, high thermal conductivity and good stability.

[0050] Example 1

[0051] (1) Use SOLIDWORK software to conduct preliminary design of the three-dimensional coil skeleton structure and complete the function and structural requirements of the parts;

[0052] (2) Use MSC software to perform stress analysis on the three-dimensional coil skeleton structure, identify stress concentration points and redundant structures, and provide a basis for structural optimization;

[0053] (3) Using digital technology, the structure is optimized according to the results of finite element simulation, stress concentration points are eliminated, redundant structures are reduced, and the overall structure is topologically optimized, so that the bearing capacity of the part structure is increased, the weight is reduced, and the local thickness is reduced, forming a hollow three-dimensional coil skeleton structure.

[0054] (4) 3D printing: After the part model design is finalized, it is digitally decomposed and the printing program is compiled. In this process, the ceramic powder needs to be screened and prepared. The powder used for the three-dimensional coil skeleton 1 is a mixed powder composed of silicon nitride powder, curing resin powder, and concentrator powder. Among them, silicon nitride powder is the main raw material for ceramic molding, accounting for 65% of the volume, curing resin powder is used as a curing agent for blank molding during 3D printing, accounting for 25% of the volume, and concentrator powder is used to concentrate laser energy, accounting for 5% of the volume, to help the melting and bonding of the curing resin to form the silicon nitride powder. The rest are auxiliary ingredients such as stabilizers and inert diluents. 3D printing selects conventional light-curing molding technology (SL), uses a mechanical scraper to accurately spread powder, and the thickness of each layer of powder is controlled at 20μm. The laser head is controlled by digital technology, and the resin powder is solidified by a laser beam. Then, the powder is spread on the molding surface and stacked layer by layer to obtain a high-precision three-dimensional coil skeleton embryo structure. Use 3D printing technology to manufacture part prototypes, and choose light-stereolithography (SL) printing technology as the printing method to ultimately form a precise part prototype structure.

[0055] (5) Degreasing and sintering: After the three-dimensional coil skeleton is printed and formed, the accuracy and size of each part basically meet the requirements of the finished product. However, in order to perform the subsequent sintering, the three-dimensional coil skeleton embryo is micro-processed and finely polished, and finally enters the high-pressure nitrogen furnace for degreasing and sintering. The degreasing is carried out in the nitrogen furnace. The embryo is heated to 700°C in a heating furnace filled with nitrogen for 1 hour and kept at normal pressure for 3 hours to melt the solidified resin and slowly precipitate. The degreasing hole 11 allows the solidified resin in the hollow structure of the part to flow out quickly, reducing the cracking of the parts caused by the uneven precipitation of the curing agent. The nitrogen protects the embryo from oxidation in a high temperature environment. After the solidified resin is completely precipitated, the temperature is raised to 1700°C within 0.5 hours, and the pressure in the nitrogen furnace is raised to 10MPa to fully sinter the silicon nitride powder together in nitrogen. The temperature is kept for more than 10 hours to promote the growth of silicon nitride grains, and finally form a silicon nitride ceramic with uniform lattice and denseness.

[0056] Example 2

[0057] (1) Use SOLIDWORK software to conduct preliminary design of the three-dimensional coil skeleton structure and complete the function and structural requirements of the parts;

[0058] (2) Use MSC software to perform stress analysis on the three-dimensional coil skeleton structure, identify stress concentration points and redundant structures, and provide a basis for structural optimization;

[0059] (3) Using digital technology, the structure is optimized according to the results of finite element simulation, stress concentration points are eliminated, redundant structures are reduced, and the overall structure is topologically optimized, so that the bearing capacity of the part structure is increased, the weight is reduced, and the local thickness is reduced, forming a hollow three-dimensional coil skeleton structure.

[0060] (4) 3D printing: After the part model design is finalized, it is digitally decomposed and the printing program is compiled. In this process, the ceramic powder needs to be screened and prepared. The powder used for the three-dimensional coil skeleton 1 is a mixed powder composed of silicon nitride powder, curing resin powder, and concentrator powder. Among them, silicon nitride powder is the main raw material for ceramic molding, accounting for 65% of the volume, curing resin powder is used as a curing agent for blank molding during 3D printing, accounting for 25% of the volume, and concentrator powder is used to concentrate laser energy, accounting for 5% of the volume, to help the melting and bonding of the curing resin to form the silicon nitride powder. The rest are auxiliary ingredients such as stabilizers and inert diluents. 3D printing selects conventional light-curing molding technology (SL), uses a mechanical scraper to accurately spread powder, and the thickness of each layer of powder is controlled at 20μm. The laser head is controlled by digital technology, and the resin powder is solidified by a laser beam. Then, the powder is spread on the molding surface and stacked layer by layer to obtain a high-precision three-dimensional coil skeleton embryo structure. Use 3D printing technology to manufacture part prototypes, and choose light-stereolithography (SL) printing technology as the printing method to ultimately form a precise part prototype structure.

[0061] (5) Degreasing and sintering: After the three-dimensional coil skeleton is printed and formed, the accuracy and size of each part basically meet the requirements of the finished product. However, in order to perform the subsequent sintering, the three-dimensional coil skeleton embryo is micro-processed and finely polished, and finally enters the high-pressure nitrogen furnace for degreasing and sintering. The degreasing is carried out in the nitrogen furnace. The embryo is heated to 650°C in a heating furnace filled with nitrogen for 1 hour and kept at normal pressure for 3 hours to melt the solidified resin and slowly precipitate. The degreasing hole 11 allows the solidified resin in the hollow structure of the part to flow out quickly, reducing the cracking of the parts caused by the uneven precipitation of the curing agent. The nitrogen protects the embryo from oxidation in a high temperature environment. After the solidified resin is completely precipitated, the temperature is raised to 1600°C within 0.5 hours, and the pressure in the nitrogen furnace is raised to 10MPa to fully sinter the silicon nitride powder together in nitrogen. The temperature is kept for more than 10 hours to promote the growth of silicon nitride grains, and finally form a silicon nitride ceramic with uniform lattice and denseness.

[0062] Example 3

[0063] (1) Use SOLIDWORK software to conduct preliminary design of the three-dimensional coil skeleton structure and complete the function and structural requirements of the parts;

[0064] (2) Use MSC software to perform stress analysis on the three-dimensional coil skeleton structure, identify stress concentration points and redundant structures, and provide a basis for structural optimization;

[0065] (3) Using digital technology, the structure is optimized according to the results of finite element simulation, stress concentration points are eliminated, redundant structures are reduced, and the overall structure is topologically optimized, so that the bearing capacity of the part structure is increased, the weight is reduced, and the local thickness is reduced, forming a hollow three-dimensional coil skeleton structure.

[0066] (4) 3D printing: After the part model design is finalized, it is digitally decomposed and the printing program is compiled. In this process, the ceramic powder needs to be screened and prepared. The powder used for the three-dimensional coil skeleton 1 is a mixed powder composed of silicon nitride powder, curing resin powder, and concentrator powder. Among them, silicon nitride powder is the main raw material for ceramic molding, accounting for 70% by volume, curing resin powder is used as a curing agent for blank molding during 3D printing, accounting for 25% by volume, and concentrator powder is used to concentrate laser energy, accounting for 5% by volume, to help the melting and bonding of the curing resin to the silicon nitride powder molding, and then added as auxiliary ingredients such as stabilizers and inert diluents; 3D printing selects conventional light-curing molding technology (SL), uses a mechanical scraper to accurately spread powder, and the thickness of each layer of powder is controlled at 15μm. The laser head is controlled by digital technology, and the resin powder is solidified by a laser beam. Then, powder is spread on the molding surface and stacked layer by layer to obtain a high-precision three-dimensional coil skeleton embryo structure. Use 3D printing technology to manufacture part prototypes, and choose light-stereolithography (SL) printing technology as the printing method to ultimately form a precise part prototype structure.

[0067] (5) Degreasing and sintering: After the three-dimensional coil skeleton is printed and formed, the accuracy and size of each part basically meet the requirements of the finished product. However, in order to perform the subsequent sintering, the three-dimensional coil skeleton embryo is micro-processed and finely polished, and finally enters the high-pressure nitrogen furnace for degreasing and sintering. The degreasing is carried out in the nitrogen furnace. The embryo is heated to 600°C in a heating furnace filled with nitrogen for 1 hour and kept at normal pressure for 4 hours to melt the solidified resin and slowly precipitate. The degreasing hole 11 allows the solidified resin in the hollow structure of the part to flow out quickly, reducing the cracking of the parts caused by the uneven precipitation of the curing agent. The nitrogen protects the embryo from oxidation in a high temperature environment. After the solidified resin is completely precipitated, the temperature is raised to 1650°C within 0.5 hours, and the pressure in the nitrogen furnace is raised to 10MPa to fully sinter the silicon nitride powder together in nitrogen. The temperature is kept for more than 10 hours to promote the growth of silicon nitride grains, and finally form a silicon nitride ceramic with uniform lattice and denseness.

[0068] Example 4

[0069] (1) Use SOLIDWORK software to conduct preliminary design of the three-dimensional coil skeleton structure and complete the function and structural requirements of the parts;

[0070] (2) Use MSC software to perform stress analysis on the three-dimensional coil skeleton structure, identify stress concentration points and redundant structures, and provide a basis for structural optimization;

[0071] (3) Using digital technology, the structure is optimized according to the results of finite element simulation, stress concentration points are eliminated, redundant structures are reduced, and the overall structure is topologically optimized, so that the bearing capacity of the part structure is increased, the weight is reduced, and the local thickness is reduced, forming a hollow three-dimensional coil skeleton structure.

[0072] (4) 3D printing: After the part model design is finalized, it is digitally decomposed and the printing program is compiled. In this process, the ceramic powder needs to be screened and prepared. The powder used for the three-dimensional coil skeleton 1 is a mixed powder composed of silicon nitride powder, curing resin powder, and concentrator powder. Among them, silicon nitride powder is the main raw material for ceramic molding, accounting for 60% by volume, curing resin powder is used as a curing agent for blank molding during 3D printing, accounting for 30% by volume, and concentrator powder is used to concentrate laser energy, accounting for 5% by volume to help the melting and bonding of the curing resin to form the silicon nitride powder. The rest are auxiliary ingredients such as stabilizers and inert diluents. 3D printing selects conventional light-curing molding technology (SL), uses a mechanical scraper to accurately spread powder, and the thickness of each layer of powder is controlled at 18μm. The laser head is controlled by digital technology, and the resin powder is solidified by a laser beam. Then, the powder is spread on the molding surface and stacked layer by layer to obtain a high-precision three-dimensional coil skeleton embryo structure. Use 3D printing technology to manufacture part prototypes, and choose light-stereolithography (SL) printing technology as the printing method to ultimately form a precise part prototype structure.

[0073] (5) Degreasing and sintering: After the three-dimensional coil skeleton is printed and formed, the accuracy and size of each part basically meet the requirements of the finished product. However, in order to perform the subsequent sintering, the three-dimensional coil skeleton embryo is micro-processed and finely polished, and finally enters the high-pressure nitrogen furnace for degreasing and sintering. The degreasing is carried out in the nitrogen furnace. The embryo is heated to 620°C in a heating furnace filled with nitrogen for 1 hour and kept at normal pressure for 3.5 hours to melt the solidified resin and slowly precipitate. The degreasing hole 11 allows the solidified resin in the hollow structure of the part to flow out quickly, reducing the cracking of the parts caused by the uneven precipitation of the curing agent. The nitrogen protects the embryo from oxidation in a high temperature environment. After the solidified resin is completely precipitated, the temperature is raised to 1630°C within 0.5 hours, and the pressure in the nitrogen furnace is raised to 10MPa to fully sinter the silicon nitride powder together in nitrogen. The temperature is kept for more than 10 hours to promote the growth of silicon nitride grains, and finally form a silicon nitride ceramic with uniform lattice and denseness.

[0074] Example 5

[0075] (1) Use SOLIDWORK software to conduct preliminary design of the three-dimensional coil skeleton structure and complete the function and structural requirements of the parts;

[0076] (2) Use MSC software to perform stress analysis on the three-dimensional coil skeleton structure, identify stress concentration points and redundant structures, and provide a basis for structural optimization;

[0077] (3) Using digital technology, the structure is optimized according to the results of finite element simulation, stress concentration points are eliminated, redundant structures are reduced, and the overall structure is topologically optimized, so that the bearing capacity of the part structure is increased, the weight is reduced, and the local thickness is reduced, forming a hollow three-dimensional coil skeleton structure.

[0078] (4) 3D printing: After the part model design is finalized, it is digitally decomposed and the printing program is compiled. In this process, the ceramic powder needs to be screened and prepared. The powder used for the three-dimensional coil skeleton 1 is a mixed powder composed of silicon nitride powder, curing resin powder, and concentrator powder. Among them, silicon nitride powder is the main raw material for ceramic molding, accounting for 62% by volume, curing resin powder is used as a curing agent for blank molding during 3D printing, accounting for 28% by volume, and concentrator powder is used to concentrate laser energy, accounting for 5% by volume, to help the melting and bonding of the curing resin to form the silicon nitride powder. The rest are auxiliary ingredients such as stabilizers and inert diluents. 3D printing selects conventional light-curing molding technology (SL), uses a mechanical scraper to accurately spread powder, and the thickness of each layer of powder is controlled at 16μm. The laser head is controlled by digital technology, and the resin powder is solidified by a laser beam. Then, the powder is spread on the molding surface and stacked layer by layer to obtain a high-precision three-dimensional coil skeleton embryo structure. Use 3D printing technology to manufacture part prototypes, and choose light-stereolithography (SL) printing technology as the printing method to ultimately form a precise part prototype structure.

[0079] (5) Degreasing and sintering: After the three-dimensional coil skeleton is printed and formed, the accuracy and size of each part basically meet the requirements of the finished product. However, in order to perform the subsequent sintering, the three-dimensional coil skeleton embryo is micro-processed and finely polished, and finally enters the high-pressure nitrogen furnace for degreasing and sintering. The degreasing is carried out in the nitrogen furnace. The embryo is heated to 680°C in a heating furnace filled with nitrogen for 1 hour and kept at normal pressure for 4 hours to melt the solidified resin and slowly precipitate. The degreasing hole 11 allows the solidified resin in the hollow structure of the part to flow out quickly, reducing the cracking of the parts caused by the uneven precipitation of the curing agent. The nitrogen protects the embryo from oxidation in a high temperature environment. After the solidified resin is completely precipitated, the temperature is raised to 1680°C within 0.5 hours, and the pressure in the nitrogen furnace is raised to 10MPa to fully sinter the silicon nitride powder together in nitrogen. The temperature is kept for more than 10 hours to promote the growth of silicon nitride grains, and finally form a silicon nitride ceramic with uniform lattice and denseness.

[0080] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A 3D printed ceramic hollow three-dimensional coil skeleton structure, characterized in that: The three-dimensional coil skeleton (1) comprises a cylindrical barrel structure, and the three-dimensional coil skeleton (1) is provided with coaxial mounting holes (6) along its length direction; The three-dimensional coil skeleton (1) is a hollow skeleton structure, which comprises a hollow transverse support (14) and a hollow longitudinal support (15); the hollow transverse support (14) and the hollow longitudinal support (15) are perpendicular to each other, and the hollow transverse support (14) and the hollow longitudinal support (15) are both arranged on a radial surface of the three-dimensional coil skeleton (1); An upper end surface support (7) and a lower end surface support (13) are respectively provided on two end surfaces of the three-dimensional coil skeleton (1), and an annular middle support (12) is provided on the body of the three-dimensional coil skeleton (1); The upper end surface support (7) and the lower end surface support (13) are both provided with an XY winding groove (9), and the XY winding groove (9) on the upper end surface support (7) is connected to the XY winding groove (9) on the lower end surface support (13); The three-dimensional coil skeleton structure is made by sintering silicon nitride ceramic material.

2. A 3D printed ceramic hollow three-dimensional coil skeleton structure according to claim 1, characterized in that: A positioning pin hole (5) is provided on the inner side wall of the mounting hole (6).

3. A 3D printed ceramic hollow three-dimensional coil skeleton structure according to claim 1, characterized in that: A plurality of degreasing holes (11) are provided in the three-dimensional coil skeleton (1), the degreasing holes (11) are arranged along the length direction of the three-dimensional coil skeleton (1), and the two ends of the degreasing holes (11) are respectively arranged on the upper end surface support (7) and the lower end surface support (13).

4. A 3D printed ceramic hollow three-dimensional coil skeleton structure according to claim 3, characterized in that: The degreasing holes (11) are arranged in equal parts along the circumference of the three-dimensional coil skeleton (1).

5. A 3D printed ceramic hollow three-dimensional coil skeleton structure according to claim 1, characterized in that: The XY winding grooves (9) are arranged in two groups, each group comprising two symmetrical XY winding grooves (9).

6. A 3D printed ceramic hollow three-dimensional coil skeleton structure according to claim 5, characterized in that: The end of the XY winding groove (9) comprises a wire accommodating groove (16) and a wire passing groove (17); the wire passing groove (17) is in communication with the wire accommodating groove (16) and the outer end surface of the three-dimensional coil skeleton (1); the width of the wire accommodating groove (16) is greater than the width of the wire passing groove (17).

7. A 3D printed ceramic hollow three-dimensional coil skeleton structure according to claim 1, characterized in that: The wire accommodating grooves (16) at both ends of an XY winding groove (9) are symmetrically arranged relative to the center point of the XY winding groove (9).

8. A method for preparing the 3D printed ceramic hollow three-dimensional coil skeleton structure according to claim 1, characterized in that: The following steps are involved: Step 1, designing a three-dimensional coil skeleton structure; Step 2, performing stress analysis on the three-dimensional coil skeleton structure by finite element simulation technology; Step 3, optimizing the three-dimensional coil skeleton structure through force analysis structure; Step 4, printing a three-dimensional coil skeleton structure blank by photocuring molding technology; the powder used in the photocuring molding technology is a mixed powder composed of silicon nitride powder, curing resin powder and concentrator powder; Step 5: Degreasing and sintering the printed three-dimensional coil skeleton structure blank to complete the preparation of the three-dimensional coil skeleton structure.

9. The preparation method according to claim 8, characterized in that: In step 4, in the photo-curing molding technology manufacturing method, a stabilizer and an inert diluent are added to the mixed powder; during the printing process of the blank, the mixed powder layer thickness is 10-20 μm.

10. The preparation method according to claim 8, characterized in that In step 4, the degreasing and sintering process is as follows: placing the three-dimensional coil skeleton structure blank in a heating furnace, keeping it at 600-700° C. for 3-4 hours; and then keeping it at 1600-1700° C. for more than 10 hours.