A method for preparing a catalyst using red mud as raw material and a process for systematically treating sewage

By preparing red mud into ceramics with Fenton reaction and photocatalytic functions, the environmental pollution problems caused by red mud accumulation are solved, efficient treatment of sewage and effective utilization of iron elements are achieved, and treatment efficiency and environmental protection effect are significantly improved. .

CN116474776BActive Publication Date: 2024-11-01BAISE UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310614691.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-29
Publication Date
2024-11-01
Estimated Expiration
2043-05-29

AI Technical Summary

Technical Problem

The large accumulation of red mud leads to environmental pollution, and the prior art fails to effectively utilize the iron element in it, and the processing capacity of the photocatalyst is limited, especially under high temperature and high pressure conditions.

Method used

The red mud is prepared into ceratops. Through Fenton reaction and photocatalytic action, iron trioxide and titanium dioxide are used to combine iron powder and sulfur powder to form ceratops with Fenton reaction, photocatalysis and adsorption functions, which are used to treat wastewater. .

Benefits of technology

It realizes effective degradation of sewage and adsorption of heavy metals, reduces the generation of pollutants, improves treatment efficiency, and is sustainable in use of ceramites, which is of environmental protection significance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116474776B_ABST
    Figure CN116474776B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of solid waste recycling and water pollution treatment, and specifically relates to a method for preparing a catalyst using red mud as a raw material and a process for systematically treating sewage. The purpose of the present invention is to provide a method for preparing a catalyst using red mud as a raw material, and a process for systematically treating sewage. The basic principle is to use ferric oxide and titanium oxide (in the form of calcium titanate) in red mud to convert ferric oxide in red mud into trivalent iron that can be used for Fenton reaction, and titanium dioxide in red mud is used for photocatalysis, and red mud is prepared into a catalyst in the form of ceramsite, and red mud washing liquid and other compounds are added at the same time, so that the red mud is finally converted into a catalyst having the functions of Fenton reaction, photocatalysis and adsorption for triple treatment of organic sewage, so as to achieve the purpose of treating waste with waste. The process has obvious environmental protection significance, strong operability, and good practical significance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of solid waste recycling and water pollution treatment, and specifically relates to a method for preparing a catalyst using red mud as a raw material and a process for systematically treating sewage. Technical Background

[0002] my country is a major producer of alumina, with an annual output of more than 1 million tons. For every ton of alumina produced, 1 to 2 tons of red mud are produced. With the expansion of the aluminum industry and the reduction of bauxite grades, the output of red mud will increase year by year, which puts enormous pressure on the environment. At present, the main methods of disposing red mud are open-air damming and open-air stacking, which not only occupies a large amount of land resources, but also causes serious pollution to the surrounding atmosphere, water, soil, microorganisms and other environments. In addition, long-term stacking treatment poses a safety hazard to the local environment.

[0003] Red mud is an industrial solid waste discharged after alumina is extracted from bauxite. It contains a large amount of iron oxide and has a reddish appearance. The production process of alumina mainly depends on the silicon-aluminum ratio of the bauxite. For high-silicon bauxite with an aluminum-silicon ratio of 3 to 5, a sintering process is generally used to refine alumina. For low-aluminum silicate with an aluminum-silicon ratio greater than 7, the Bayer process is generally used to refine alumina. The Bayer process is mainly used for alumina production in my country. Although the processes are different, the main components of the red mud obtained are basically the same, all containing hydrated garnet (3CaO·Al2O3·3SiO2·xH2O), hydroxysodalite (Na8Al6Si6O 24 (OH2)), calcium titanate (CaTiO3), calcite (CaCO3) and hematite (Fe2O3). In addition, the Bayer process also has a small amount of hydrated sodium aluminosilicate, hydrated sodium aluminosilicate and diaspore, while the sintering method has various types of dicalcium silicate and sodium aluminosilicate.

[0004] Red mud has the characteristics of complex composition, strong alkalinity and high iron content, among which iron mainly exists in the form of ferric oxide. Taking Guangxi as an example, the iron oxide content in red mud is not less than 30%. The main elements in red mud are Fe (14% to 45%), Al (5% to 14%), Si (1% to 9%), Ti (2% to 12%), and Na (1% to 9%). At the same time, red mud sometimes contains trace amounts of As, Cr, Hg, Cd and other harmful heavy metal elements due to different sources. Red mud also has the characteristics of porous materials such as good particle dispersion and large specific surface area, and good stability in solution, which makes it used in building materials, metallurgy, environmental protection and other fields. For example, a Chinese invention patent (CN202211249876.0) discloses a method for using red mud in cement production with zero carbon emissions; an authorized invention patent (CN202210024994.5) provides a method for selectively leaching rare earth elements from red mud; an invention patent (CN202211109831.3) discloses a process for treating benzene-containing wastewater with red mud and chlorine. The invention uses red mud to adsorb benzene-containing wastewater, and then treats the red mud with chlorine to obtain a product, thus achieving red mud, benzene-containing wastewater treatment. The resource utilization of three kinds of wastes, wastewater and chlorine, does not mention the environmental protection utilization of important elements such as iron and titanium in red mud; China's invention patent (CN202211117021.2) discloses a process for treating 2-naphthol production wastewater with red mud. The invention utilizes the acidity of 2-naphthol production wastewater and the high alkalinity of red mud to achieve the purpose of treating waste with waste; the same China's invention patent (CN202211106578.6) discloses a synergistic treatment of difficult-to-degrade organic waste and red mud. The invention uses supercritical oxidation to treat refractory organic waste and red mud in a coordinated manner. The red mud is dealkalized while leaching out metal components. Aluminum oxide and iron oxide in the metal components can be used as catalysts to promote the degradation of organic waste. At the same time, the carbon dioxide decomposed from organic matter can be absorbed by red mud, thereby achieving coordinated treatment of the two pollutants. The Chinese invention patent (CN202110998703.8) discloses a red mud-based composite photocatalytic material loaded with flaky carbon nitride and a preparation method thereof. The method is based on a flaky gC- (3) A Fe-(2)O-(3) / Co-(3)O-(4) heterojunction structure is formed on N-(4), which slows down the recombination rate of electrons and holes and increases the photocatalytic degradation efficiency of the material. The authorized invention patent (CN201910347426.7) is a preparation method and application of a red mud-based composite photocatalyst. The method is to use red mud powder and melamine in combination to obtain a red mud / C-3N-4 composite photocatalyst. The composite photocatalyst can catalytically degrade antibiotics in wastewater under visible light conditions.Regarding the environmental protection utilization of important elements such as iron and titanium in the above red mud, especially how to use a large amount of iron, there is no good development and utilization except for extraction. In addition, the photocatalysts developed mainly use dopants to form heterojunctions to obtain the catalytic degradation function of pollutants, or add oxygen to improve the oxidation ability of oxygen under high temperature and high pressure conditions to obtain pollutant treatment capabilities.

[0005] The invention is a preparation and utilization process of an environmentally friendly material developed on the basis of electrolytic aluminum waste slag. The red mud is first dried and ground into powder, and then added into a dilute acid solution in a certain proportion. When the raw material liquid presents brown red or yellow and the solid matter is no longer dissolved, the powder is filtered and separated, and the liquid is used as red mud washing liquid for standby use. The filtered powder slag is mixed with a certain amount of iron powder and sulfur powder until it is uniform. A certain amount of sodium carbonate or sodium bicarbonate solution is added to the mixed powder material, and the wet basis water content of the material is controlled to be about 20%. The wet material is prepared into spheres less than 10 mm, and then the surface of the spheres is sprayed with dilute acid to wet it, and then the spheres are immediately placed in a high-temperature reaction device, and the temperature is raised in stages under an inert atmosphere (isolated from oxygen), and then the temperature is lowered to 100° C. to obtain red mud ceramsite. Sewage is introduced into a degradation pool with good sunlight or ultraviolet light, ceramsite and red mud washing solution are added, the pH value is adjusted, and a certain amount of hydrogen peroxide is added to initiate the reaction. The ceramsite has three capabilities: Fenton reaction, photocatalytic degradation and adsorption; the ceramsite can continue to be used as ceramsite with adsorption and photocatalytic capabilities after treating a certain amount of solution. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing a catalyst using red mud as a raw material, and a process for systematically treating sewage. The basic principle is to utilize ferric oxide and titanium oxide (in the form of calcium titanate) in the red mud to convert the ferric oxide in the red mud into trivalent iron that can be used for the Fenton reaction, and the titanium dioxide in the red mud is used for photocatalysis, and the red mud is prepared into a catalyst in the form of ceramsite, and red mud washing liquid and other compounds are added at the same time, so that the red mud is finally converted into a catalyst having the functions of Fenton reaction, photocatalysis and adsorption for triple treatment of organic sewage, so as to achieve the purpose of treating waste with waste. The process has obvious environmental protection significance, strong operability and good practical significance.

[0007] To achieve the above purpose, the technical solution steps adopted by the present invention are as follows:

[0008] (1) Take a certain amount of red mud to measure its components and their contents, grind it into powder, and transfer it to a reactor, which is called red mud A.

[0009] (2) Add 5-30wt% hydrochloric acid or sulfuric acid to the reactor containing red mud A in step (1) to completely neutralize the alkali therein, and then continue to add the 5-30wt% hydrochloric acid or sulfuric acid to react with ferric oxide, and keep stirring for 3-6 hours until the solution completely turns brown red or brown yellow, and the pH value of the reaction system is close to neutral. (The fundamental purpose of adding hydrochloric acid or sulfuric acid in this step is to generate a trivalent iron solution to participate in the later Fenton reaction, and its basic reaction formula is:

[0010] Fe2O3+6HCl=2FeCl3+3H2O, 2Fe2O3+3H2SO4=Fe2(SO4)3+3H2O)

[0011] (3) The material in the reactor of step (2) is filtered and separated, the solution is red mud washing liquid A, and the solid material is red mud B.

[0012] (4) Add elemental refined iron powder (the iron powder is added to produce Fenton reaction with ferric chloride in red mud washing solution A and hydrogen peroxide added later to degrade organic matter) to the red mud B in step (3), and then add sulfur powder (the elemental sulfur is added to solidify ionic compounds of heavy metal mercury Hg and cadmium Cd that may be produced in the high-temperature reaction during the preparation of ceramsite, and can generate water-insoluble HgS, CdS, Cr2S3, As2S2) and mix them evenly, and then add sodium carbonate or sodium bicarbonate powder (the carbonate is added to react with the dilute acid in the subsequent steps. The technical solution of the present invention provides a chemical reaction active foaming method, which is different from the traditional ceramsite that uses aluminum powder and other foaming agents to react with water vapor. The density of the ceramsite is smaller and the adsorption capacity is stronger. Its bulk density can be stably less than 1 kg / m 3 ) and add a certain amount of clean water to ensure that the wet basis moisture content of the entire solid mixture is about 20%, which is called red mud C.

[0013] (5) The red mud C is prepared into spheres with a diameter less than 5-10 mm using a granulator, which is called red mud ceramsite A.

[0014] (6) The surface of the red mud ceramsite A is sprayed with 0.5-5wt% dilute hydrochloric acid and dilute sulfuric acid until the surface is completely wetted, and then immediately transferred into a high-temperature reactor with an inert atmosphere function, and the reactor is sealed. The air in the reactor can be replaced by an inert gas such as nitrogen and argon (the inert atmosphere is provided to protect the iron powder from oxidation).

[0015] (7) Under an inert atmosphere, the material in step (6) is heated to 117±5°C (not lower than 112°C, which is the liquefaction temperature of elemental sulfur. Elemental sulfur liquefies at this temperature in the ceramsite and flows into the nearby pores. The purpose of constant temperature is to make the elemental sulfur evenly distributed) at a rate of not more than 10°C / min, and then continued to be heated to 450±5°C (not lower than 445°C, which is the vaporization temperature of elemental sulfur. The elemental sulfur has been evenly distributed) at a rate of not more than 10°C / min. The uniform elemental sulfur reacts with mercury and cadmium at this high temperature to finally generate HgS and CdS. The time required to maintain the reaction is sufficient to ensure that the reaction is complete). Keep the temperature constant for 30-60 minutes, then raise the temperature to 900-1100°C (this temperature is the temperature for calcining the ceramsite), keep the temperature constant for 30-60 minutes, then cool to below 100°C, and then naturally cool to room temperature to obtain red mud ceramsite B. At this time, the important components of the ceramsite are TiO2, elemental iron, solidified sulfide, and silicon-aluminum oxide materials that constitute the ceramsite skeleton. (8) Prepare an organic wastewater degradation tank with aeration function (to stir the ceramsite) and ultraviolet light irradiation (the ultraviolet light can irradiate the ceramsite, so the degradation tank cannot be too deep).

[0016] (9) Add red mud washing liquid A into the degradation tank; add a certain amount of wastewater (it is necessary to calculate the molar amount of Fe in the red mud washing liquid A first, and 100-700g of wastewater with a COD mass can be added for every 1 mol of Fe. It should be noted that the present invention uses potassium dichromate K2Cr2O7 as an oxidant to determine the chemical oxygen demand, i.e., COD); add a certain amount of dilute hydrochloric acid or dilute sulfuric acid to control the pH value of the water body at 5±0.5; add ceramsite B, and then add hydrogen peroxide equivalent to 10% to 30% of the COD mass of organic pollution in the wastewater in this step (the amount of hydrogen peroxide used is reduced by 90%-70% compared with the "HJ1095-2020 Fenton Oxidation Wastewater Treatment Engineering Technical Specifications").

[0017] (10) Aeration and ultraviolet light are turned on in the degradation tank, and a batch of sewage can be treated after 1 to 12 hours of reaction.

[0018] In the process of sewage degradation, TiO2 can realize photocatalytic degradation of organic pollutants in wastewater, Fenton reagent degradation reaction, and adsorption of solid pollutants; after the elemental iron in the ceramsite is consumed (or iron powder is added to the solution at a later stage to maintain the Fenton reaction), the ceramsite will continue to have the photocatalytic degradation function.

[0019] Preferably, in step (2), after the pH value of the reaction system is close to neutral after neutralization, hydrochloric acid is added at 5.6-6.0 times the molar amount of ferric oxide in red mud A, or dilute sulfuric acid is added at 1.4-1.5 times the molar amount of ferric oxide in red mud A.

[0020] Preferably, in step (4), the amount of the refined iron powder added is 3.2-3.5 times the molar amount of ferric oxide in the red mud A.

[0021] Preferably, in step (4), the amount of sulfur powder added is 1 / 200-1 / 300 of the mass of the red mud A.

[0022] Preferably, in step (4), the amount of sodium carbonate or sodium bicarbonate powder added is 2-5wt% of the mass of the red mud A.

[0023] One of the characteristics of the present invention is the use of Fenton reaction. First, the ferric oxide in the red mud is converted into trivalent iron (Fe2(SO4)3, FeCl3) that can be used in the Fenton reaction; then the zero-valent iron (iron powder doped in ceramsite) is reacted in a solution containing H2O2. Under acidic conditions, the zero-valent iron is corroded to generate Fe 2+ The degradation mechanism is ferrous ions (Fe 2+ ) as a catalyst, and then react with the oxidant hydrogen peroxide (H2O2) to produce hydroxyl radicals (·OH); at the same time, Fe3+ undergoes a rapid redox reaction on the surface of zero-valent iron to generate Fe2+ again; ·OH has extremely strong oxidizing properties and can degrade most organic pollutants. Its mechanism reaction equation is as follows (1)-(4):

[0024] Fe 0 +2H + →Fe 2+ +H2 Formula (1)

[0025] Fe 2+ +H2O2→Fe 3+ +HO·+OH - Formula (2)

[0026] Fe 3+ +H2O2→Fe 2+ +HO·+H + Formula (3)

[0027] Fe 0 +Fe 3+ →3Fe 2+ Formula (4)

[0028] The second feature of the present invention is that titanium dioxide in red mud is used to make the prepared ceramsite have a photocatalytic effect. At the same time, the ultraviolet light used in the photocatalytic process and the hydroxyl free radicals that can be generated can effectively enhance the Fenton reaction. The Fenton reaction and photocatalysis promote each other and do not weaken each other. The inferred reaction mechanism is as follows (5)-(11):

[0029] TiO2+hv→h + +e - Formula (5)

[0030] h + +OH - →·OH Formula (6)

[0031] h + +H2O→·OH+H + Formula (7)

[0032] e - +O2→O2 - Formula (8)

[0033] O2 - +H + →H2O· Formula (9)

[0034] H2O·→O2+H2O2 formula (10)

[0035] H2O2+O2→·OH+H + +O2 Formula (11)

[0036] In general, the ceramsite prepared by the present invention has not only the common adsorption function, but also the function of providing a catalyst for catalytic degradation of organic pollutants, that is, providing elemental iron for Fenton reaction and titanium dioxide for photocatalysis. Under acidic conditions, ultraviolet light irradiation and aeration conditions, the addition of hydrogen peroxide can convert the trivalent iron in the red mud washing liquid into divalent iron, generating hydroxyl free radicals that can degrade organic pollutants; ultraviolet light irradiation can cause the floating ceramsite in the aeration process to generate hole-electron pairs, which can generate negative oxygen ions and hydroxyl free radicals with degradation function under acidic conditions and the more abundant oxygen brought by the aeration process. The basic principle diagram of the catalytic degradation function of ceramsite is shown in the figure below. Figure 1 shown.

[0037] The present invention fully considers all aspects of red mud treatment during the red mud treatment process, embodies the concept of comprehensive management and comprehensive utilization, makes full use of the iron and titanium in the red mud, considers the possible trace heavy metals in the solidified red mud, and uses it for wastewater treatment while treating the waste. The overall process needs to fully consider all steps of the treatment. The process flow diagram is shown in FIG. Figure 2 . BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 Mechanism diagram of ceramsite catalytic degradation

[0039] Figure 2 Schematic diagram of red mud-based ceramsite with degradation function and wastewater treatment process flow DETAILED DESCRIPTION

[0040] Example 1

[0041] This embodiment is described based on unit mass, i.e., per kilogram of red mud. 1 kg of red mud from a Bayer process alumina manufacturer in Baise City was taken, dried and ground, and its mass composition was analyzed as follows:

[0042]

[0043] The obtained red mud is transferred to a corrosion-resistant reactor, and about 2.55 kg of 10% (wt) hydrochloric acid solution is slowly dripped into it. During the dripping process, the reactor is gradually stirred until the reaction system is liquefied and stirred normally until the reaction system is neutral. Then 4.9 kg of 10% hydrochloric acid is added and the stirring state is maintained. The reaction is carried out for 6 hours, and the reaction liquid is generally brown-red or brown-yellow. The solid-liquid mixture in the previous step is filtered and separated to obtain the solid red mud B and the solution red mud washing liquid A for later use. The obtained red mud B is sprayed with about 125g of refined iron powder and 10g of sulfur powder (below 100 mesh), and the mixture is continuously sieved and mixed; 10g of sodium carbonate is easily mixed with 620g of clean water to obtain a sodium carbonate solution, and the sodium carbonate solution is evenly sprayed on the red mud B doped with iron powder and sulfur powder to obtain red mud C, and the red mud C is prepared into 5-10mm balls by a granulator, which are called ceramsite A; the surface of the ceramsite A is sprayed with 1.5% dilute hydrochloric acid, and then quickly transferred into a high-temperature reactor with an inert atmosphere function, the closed reactor is replaced and the air in the furnace is replaced with nitrogen, and the high-temperature furnace heating program is started, and the whole heating rate is set to 8°C / min, to 117°C, constant temperature for 60 minutes, then heated to 450°C, constant temperature for 60 minutes, then heated to 950°C, constant temperature for 60 minutes, and then cooled to below 100°C for discharge, and naturally cooled to room temperature, which is called ceramsite B. Prepare an organic wastewater degradation pool with aeration function and ultraviolet light irradiation. The amount of organic pollution that can be treated by 1kg of ceramsite prepared from red mud and the red mud washing liquid produced are as follows:

[0044] (1) Treating a certain azo dye wastewater, the water quality COD: 15000mg / L, chromaticity about 4000 times. Put about 120L into the sewage degradation tank; add red mud washing liquid A; adjust pH to 5 with 30% hydrochloric acid; add all the prepared ceramsite B; start the aeration and ultraviolet light of the reaction tank; add 1.5L of 30% hydrogen peroxide; react at room temperature for 6 hours; the effluent water quality CODCr: 330mg / L, chromaticity 37 times, after subsequent pH value and desalination treatment, it can meet the national secondary emission standard.

[0045] (2) Treatment of leachate generated by a community garbage transfer station in a certain city. The COD was 17200 mg / L and the color was about 9000 times. About 156L was put into the sewage degradation tank; red mud washing liquid A was added; 30% hydrochloric acid was used to adjust the pH to 4.5; ceramsite B was added; the aeration and ultraviolet light of the reaction tank were turned on; 1.7L of 30% hydrogen peroxide was added; the reaction was carried out at room temperature for 8 hours; the effluent COD was 6230 mg / L and the color was 80 times, meeting the requirements for biochemical water inlet.

[0046] (3) Treatment of aniline wastewater, the COD was 5100 mg / L, about 270 L was added; red mud washing liquid A was added; 30% hydrochloric acid was used to adjust the pH to 4.5; ceramsite B was added; aeration and ultraviolet light of the reaction tank were turned on; 1.7 L of 30% hydrogen peroxide was added; the reaction was carried out at room temperature for 8 hours; the COD of the effluent water was 94 mg / L, and after subsequent pH adjustment and desalination treatment, it could meet the national secondary emission standard.

[0047] Example 2

[0048] This embodiment is described based on unit mass, i.e., per kilogram of red mud. 1 kg of red mud from a Bayer process alumina manufacturer in Baise City was taken, dried and ground, and its mass composition was analyzed as follows:

[0049]

[0050]

[0051] The obtained red mud is transferred to a corrosion-resistant reactor, and about 4.42 kg of 10% (wt) sulfuric acid solution is slowly dripped into the reactor. During the dripping process, the reactor is gradually stirred until the reaction system is liquefied and stirred normally until the reaction system is neutral. Then 6.58 kg of 5% sulfuric acid (wt) is added, and the stirring state is maintained. The reaction is carried out for 6 hours, and the reaction liquid is generally brown-red or brown-yellow;

[0052] The solid-liquid mixture in the previous step is filtered and separated to obtain a solid red mud B and a solution red mud washing liquid A for later use. The obtained red mud B is sprayed with about 125g of refined iron powder and 10g of sulfur powder (below 100), and the mixture is continuously sieved and mixed; 12g of sodium bicarbonate is dissolved in 620g of clean water to obtain a sodium bicarbonate solution, and the sodium bicarbonate solution is evenly sprayed on the red mud B doped with iron powder and sulfur powder to obtain red mud C, and the red mud C is prepared into 5-10mm balls by a granulator, which are called ceramsite A; the surface of ceramsite A is sprayed with 0.5% dilute sulfuric acid, and then quickly transferred into a high-temperature reactor with an inert atmosphere function, the closed reactor is replaced and the air in the furnace is replaced with nitrogen, and the high-temperature furnace heating program is started, and the whole heating rate is set to 8℃ / min, to 117℃, constant temperature for 60 minutes, then heated to 450℃, constant temperature for 60 minutes, then heated to 950℃, constant temperature for 60 minutes, and then cooled to below 100℃ to discharge, and naturally cooled to room temperature, which is called ceramsite B. Prepare an organic wastewater degradation pool with aeration function and ultraviolet light irradiation. The amount of organic pollution that can be treated by 1kg of ceramsite prepared from red mud and the red mud washing liquid produced are as follows:

[0053] (1) Treating a certain azo dye wastewater, the water quality COD: 15000mg / L, the chromaticity is about 4000 times. Put about 130L into the sewage degradation tank; add red mud washing liquid A; adjust the pH to 5 with 10% sulfuric acid; add ceramsite B; start the aeration and ultraviolet light of the reaction tank; add 1.6L of 30% hydrogen peroxide by mass; react at room temperature for 6 hours; the effluent water quality COD: 317mg / L, chromaticity 36 times, after subsequent pH value and desalination treatment, it can meet the national secondary emission standard.

[0054] (2) Treatment of leachate generated by a community garbage transfer station in a certain city. The COD was 17200 mg / L and the color was about 9000 times. About 163L was put into the sewage degradation tank; red mud washing liquid A was added; 10% hydrochloric acid was used to adjust the pH to 4.5; ceramsite B was added; the aeration and ultraviolet light of the reaction tank were turned on; 1.8L of 30% hydrogen peroxide was added; the reaction was carried out at room temperature for 8 hours; the effluent COD was 6192 mg / L and the color was 76 times, meeting the requirements for biochemical water inlet.

[0055] (3) Treatment of aniline wastewater, the COD was 5100 mg / L, about 290 L was added; red mud washing liquid A was added; 10% sulfuric acid was used to adjust the pH to 4.5; expanded clay B was added; aeration and ultraviolet light were turned on in the reaction tank; 1.8 L of 30% by mass hydrogen peroxide was added; the reaction was carried out at room temperature for 8 hours; the effluent COD was 91 mg / L, and after subsequent pH adjustment and desalination treatment, it could meet the national secondary emission standard.

[0056] The description of the above embodiments is to facilitate the understanding and use of the invention by those skilled in the art. The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a catalyst using red mud as raw material, characterized in that The preparation steps are as follows: (1) Take a certain amount of red mud to measure its components and their contents, grind it into powder, and transfer it to a reactor, which is called red mud A; (2) adding 5-30 wt% hydrochloric acid or sulfuric acid to the reaction kettle containing red mud A in step (1) to completely neutralize the alkali therein, and then continuing to add the 5-30 wt% hydrochloric acid or sulfuric acid to react with ferric oxide, and maintaining the reaction for 3-6 hours under stirring until the solution completely turns brown-red or brown-yellow, at which time the pH value of the reaction system is neutral; (3) filtering and separating the materials in the reactor of step (2), wherein the solution is red mud washing liquid A, and the solid material is red mud B; (4) Add elemental refined iron powder and sulfur powder to the red mud B in step (3) and mix them evenly. Then, add sodium carbonate or sodium bicarbonate powder and a certain amount of clean water to ensure that the wet basis moisture content of the entire solid mixture is 20%, which is called red mud C; (5) The red mud C is prepared into spheres with a diameter less than 5-10 mm by a granulator, which are called red mud ceramsite A; (6) Spraying the surface of the red mud ceramsite A with 0.5-5wt% dilute hydrochloric acid or dilute sulfuric acid until the surface is completely wetted, and then immediately transferring it into a high-temperature reactor with an inert atmosphere function, and sealing the reactor; (7) Under an inert atmosphere, the material in step (6) is heated to 117±5°C at a rate of not more than 10°C / min, maintained at the temperature for 30-60 minutes, then heated to 450±5°C at a rate of not more than 10°C / min, maintained at the temperature for 30-60 minutes, then heated to 900-1100°C, maintained at the temperature for 30-60 minutes, then cooled to below 100°C, and then naturally cooled to room temperature to obtain red mud ceramsite B.

2. A method for preparing a catalyst using red mud as raw material as claimed in claim 1, characterized in that: In step (2), after the pH value of the reaction system is close to neutral after neutralization, hydrochloric acid is added at 5.6-6.0 times the molar amount of ferric oxide in the red mud A, or dilute sulfuric acid is added at 1.4-1.5 times the molar amount of ferric oxide in the red mud A.

3. The method for preparing a catalyst using red mud as raw material according to claim 1, characterized in that: In step (4), the amount of the refined iron powder added is 3.2-3.5 times the molar amount of ferric oxide in the red mud A.

4. The method for preparing a catalyst using red mud as raw material according to claim 1, characterized in that: In step (4), the amount of sulfur powder added is 1 / 200-1 / 300 of the mass of the red mud A.

5. The method for preparing a catalyst using red mud as raw material according to claim 1, characterized in that: In step (4), the amount of sodium carbonate or sodium bicarbonate powder added is 2-5wt% of the mass of the red mud A.

6. A process for systematically treating wastewater using red mud as raw material, characterized in that Here are the steps: (1) Take a certain amount of red mud, measure its components and their contents, grind it into powder, and transfer it to a reactor, which is called red mud A; (2) adding 5-30 wt% hydrochloric acid or sulfuric acid to the reaction kettle containing red mud A in step (1) to completely neutralize the alkali therein, and then continuing to add the 5-30 wt% hydrochloric acid or sulfuric acid to react with ferric oxide, and maintaining the reaction for 3-6 hours under stirring until the solution completely turns brown-red or brown-yellow, at which time the pH value of the reaction system is neutral; (3) filtering and separating the materials in the reactor of step (2), wherein the solution is red mud washing liquid A, and the solid material is red mud B; (4) Add elemental refined iron powder and sulfur powder to the red mud B in step (3) and mix them evenly. Then, add sodium carbonate or sodium bicarbonate powder and a certain amount of clean water to ensure that the wet basis moisture content of the entire solid mixture is 20%, which is called red mud C; (5) The red mud C is prepared into spheres with a diameter less than 5-10 mm by a granulator, which are called red mud ceramsite A; (6) Spraying the surface of the red mud ceramsite A with 0.5-5wt% dilute hydrochloric acid or dilute sulfuric acid until the surface is completely wetted, and then immediately transferring it into a high-temperature reactor with an inert atmosphere function, and sealing the reactor; (7) Under an inert atmosphere, the material in step (6) is heated to 117±5°C at a rate of no more than 10°C / min, maintained at the constant temperature for 30-60 minutes, then heated to 450±5°C at a rate of no more than 10°C / min, maintained at the constant temperature for 30-60 minutes, then heated to 900-1100°C, maintained at the constant temperature for 30-60 minutes, then cooled to below 100°C, and then naturally cooled to room temperature to obtain red mud ceramsite B; (8) Prepare an organic wastewater degradation pool with aeration function and ultraviolet light irradiation; (9) Add red mud washing liquid A into the degradation tank, add a certain amount of wastewater, add a certain amount of dilute hydrochloric acid or dilute sulfuric acid, control the pH value of the water body at 5±0.5, then add red mud ceramsite B, and finally add hydrogen peroxide equivalent to 10%~30% of the mass of organic pollution COD in the wastewater; (10) Turn on aeration and UV light in the degradation tank and let the reaction take 1 to 12 hours to treat a batch of sewage.

7. A process for systematically treating sewage using red mud as raw material as claimed in claim 6, characterized in that: In step (2), after the pH value of the reaction system is close to neutral after neutralization, hydrochloric acid is added at 5.6-6.0 times the molar amount of ferric oxide in the red mud A, or dilute sulfuric acid is added at 1.4-1.5 times the molar amount of ferric oxide in the red mud A.

8. A process for systematically treating sewage using red mud as raw material as claimed in claim 6, characterized in that: In step (4), the amount of the refined iron powder added is 3.2-3.5 times the molar amount of ferric oxide in the red mud A.

9. A process for systematically treating sewage using red mud as raw material as claimed in claim 6, characterized in that: In step (4), the amount of sulfur powder added is 1 / 200-1 / 300 of the mass of the red mud A.

10. A process for systematically treating sewage using red mud as raw material as claimed in claim 6, characterized in that: In step (4), the amount of sodium carbonate or sodium bicarbonate powder added is 2-5wt% of the mass of the red mud A.