A preparation method of nano calcium carbonate
By adding high concentration of soluble salt compounds and adjusting the reaction temperature during the preparation of nano calcium carbonate, the pollution and particle size control problems caused by crystal form control agents in the prior art are solved, and nanocarbonic acid without adding crystal form control agents is realized Calcium preparation, and nano calcium carbonate particles with good dispersion of 80-200nm are obtained, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202310242653.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-14
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-03-14
AI Technical Summary
The existing nano calcium carbonate preparation method requires the addition of crystal form control agents, which leads to wastewater pollution and difficulty in controlling particle size, and it is difficult to obtain nano calcium carbonate particles above 100 nm.
High concentration of soluble salt compounds are used to affect the nucleation and growth of calcium carbonate precipitated particles during the carbonization reaction, and 80-200nm of cubic and rod-shaped nano calcium carbonate is obtained by adjusting the reaction temperature, and no crystal form control agent is required.
It realizes the preparation of nano-calcium carbonate with non-toxic and harmless and simple steps. It can reuse the filtrate, reduce the treatment cost, and obtain nano-calcium carbonate particles with good dispersion, which is suitable for industrial production.
Smart Images

Figure CN116477653B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of inorganic nano material preparation, and mainly relates to a preparation method of nano calcium carbonate using a new process. Background Art
[0002] Calcium carbonate is mainly used in the fields of coatings, rubber, plastics, inks, papermaking, cosmetics, and medicine. It has the advantages of low cost, high performance, non-toxicity, good color, and high whiteness. It is a high-quality filler and white pigment. Compared with ordinary calcium carbonate products, nano calcium carbonate has the characteristics of fine particles, large specific surface area, high reinforcement, and good thixotropy. It is one of the nano materials that can be mass-produced and applied at present. It can partially replace the expensive white carbon black and titanium dioxide, and has broad market prospects.
[0003] In the industrial production process of nano calcium carbonate, in order to obtain nanometer-level particle size, it is necessary to add crystal form control agent, and the commonly used crystal form control agent of the industry such as inorganic acid (sulfuric acid, acetic acid, phosphoric acid and pyrophosphoric acid etc.) and salt (aluminum sulfate, zinc sulfate and sodium tripolyphosphate etc.) and organic sugar, polyols, hydroxycarboxylic acid and its salt and its mixture thereof are mostly used. Because nano calcium carbonate can produce a large amount of waste water in the solid-liquid separation process, the crystal form control agent contained in these waste waters can affect the morphology of product when recycling, and the sugar crystal form control agent can ferment in aqueous solution, makes bacterial propagation and produces unpleasant smell. And its particle size of the nano calcium carbonate prepared by the above method is mostly below 100nm, and it is difficult to obtain the nano calcium carbonate particles with a size of more than 100nm.
[0004] Chinese invention patent CN114314629B discloses a method for preparing nano calcium carbonate based on surface potential control. The surface potential of the crystal is determined by the charge on the surface. By introducing positively charged homologous calcium ions to increase the number of calcium ions on the crystal surface, the surface potential is increased. Crystals with high positive potential repel each other to maintain the stability of the system. With this process, the filtrate can be supplemented with calcium oxide to form a saturated solution for repeated use, but it is still difficult to obtain nano calcium carbonate particles with a size of more than 100nm.
[0005] In view of this, the present invention provides a non-toxic and harmless preparation method of nano calcium carbonate with extremely simple steps, which not only does not require the addition of a crystal form control agent, but also can achieve the reuse of the filtrate, and can obtain nano calcium carbonate with a size distribution of 80-200nm and obtain rod-shaped nano calcium carbonate by adjusting the reaction temperature. Summary of the invention
[0006] The object of the present invention is to provide a method for preparing nano calcium carbonate in view of the deficiencies of the prior art. The method is extremely simple and suitable for industrial production, and can obtain cubic nano calcium carbonate and rod-shaped nano calcium carbonate with good dispersibility and a size distribution of 80-200 nm without adding a crystal form control agent. The present invention finds that when a high concentration of soluble salt compounds is added to lime milk, during the carbonization reaction, the high concentration of ions present in the solution can affect the nucleation and growth process of calcium carbonate precipitation particles during the carbonization process.
[0007] The technical solution adopted by the present invention to solve the technical problem is as follows:
[0008] A method for preparing nano calcium carbonate comprises digesting a substance containing calcium oxide to obtain lime milk, and then subjecting the lime milk to carbonization reaction with a gas containing carbon dioxide after aging to obtain nano calcium carbonate after treatment, wherein a soluble salt is also added during the reaction.
[0009] Preferably, the calcium oxide content in the substance containing calcium oxide is not less than 90%; more preferably, the substance containing calcium oxide is quicklime or calcium oxide, and more preferably, quicklime is obtained by calcining and decomposing limestone.
[0010] Preferably, the soluble salt is added at any time point before the carbonization reaction of the preparation method; more preferably, the soluble salt is added during digestion, or after digestion is completed, or before the carbonization reaction. More preferably, the soluble salt is added as follows:
[0011] a. dissolving a soluble salt in water to obtain a soluble salt solution, digesting the substance containing calcium oxide with the soluble salt solution, and performing subsequent steps;
[0012] or b. digesting the substance containing calcium oxide and water to obtain lime milk, adding a soluble salt to the lime milk and dissolving it, and performing subsequent steps;
[0013] or c. digesting the substance containing calcium oxide and water to obtain lime milk and aging it, adding a soluble salt to the aged lime milk and dissolving it, and then carrying out the subsequent steps.
[0014] Preferably, the soluble salt is at least one of a soluble sodium salt, a soluble potassium salt, and a soluble lithium salt, and more preferably, the soluble salt is at least one of sodium chloride, sodium sulfate, sodium nitrate, sodium phosphate, and sodium hexametaphosphate. The technical solution can further reduce costs while achieving the technical effect.
[0015] Preferably, the ratio of the total amount of the soluble salt added to the amount of calcium oxide in the substance containing calcium oxide is between 0.5-4:1, preferably between 1-3:1, and most preferably between 1.5-2:1.
[0016] Preferably, the water temperature during digestion is controlled at 30-80° C., preferably 40-70° C., and most preferably 50-60° C. The technical solution can further ensure that calcium oxide fully reacts with water, reducing interference with the product in the later stage.
[0017] Preferably, the mass ratio of the digestion water to the calcium oxide in the substance containing calcium oxide is between 4:1-6:1, but before the carbonization reaction, the concentration of calcium hydroxide in the lime milk is adjusted to be no higher than 1.5 mol / L, and the more preferred concentration of calcium hydroxide is between 0.8 and 1.5 mol / L. The technical solution can further ensure that the viscosity of the reaction system is not too large, avoiding a significant impact on the morphology of the product; at the same time, considering the economic cost factor, the range of 0.8 to 1.5 mol / L is more suitable.
[0018] Preferably, the dosage of the gas containing carbon dioxide is calculated as the minute ventilation volume (L / min) of carbon dioxide and the amount of calcium oxide in the substance containing calcium oxide in a ratio of 0.1 to 1:1.
[0019] Preferably, for cubic nano-calcium carbonate, the carbonization reaction temperature is 5-30°C, preferably 10-25°C, and most preferably 15-20°C.
[0020] Preferably, for rod-shaped nano-calcium carbonate, the carbonization reaction temperature is 30-60°C, preferably 35-55°C, and most preferably 40-50°C.
[0021] Preferably, the treatment includes surface treatment, and the surface treatment is surface coating treatment using a coating agent. More preferably, the coating agent is a conventional coating agent such as sodium stearate. More preferably, the amount of the coating agent is 3-4% of the mass of calcium carbonate. More preferably, the surface treatment is carried out at 70-85°C.
[0022] Preferably, the treatment further includes conventional treatment steps such as filtration, washing, and drying.
[0023] Preferably, the preparation method can also use limestone as raw material, calcine it to decompose into quicklime calcium oxide, then digest and age it, then introduce gas containing carbon dioxide to carry out carbonization reaction, and stop aeration after continuing aeration for 15 minutes when the solution pH=7, and obtain nano calcium carbonate after surface treatment, filtration, washing and drying; soluble salt is also added during the reaction process.
[0024] Preferably, the preparation method specifically comprises the following steps:
[0025] 1) water at a certain temperature and a substance containing calcium oxide are subjected to a digestion reaction in a certain ratio to obtain lime milk;
[0026] 2) Add a certain amount of soluble salts to the lime milk;
[0027] 3) After aging the lime milk for 24 hours, filtering and removing slag, introducing carbon dioxide or kiln gas containing carbon dioxide into the obtained refined lime milk for carbonization reaction;
[0028] 4) When the solution pH = 7, continue to ventilate for 15 minutes, then stop ventilating, raise the temperature to 70-85°C, and add sodium stearate coating agent for surface coating treatment;
[0029] 5) The coated calcium carbonate is filtered, washed three times and then dried to obtain nano calcium carbonate.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) In the present invention, it is not necessary to add a crystal form control agent, and the growth of calcium carbonate particles can be controlled by adding salts. The salt-containing filtrate produced in the subsequent filter pressing process can be reused, which reduces the processing cost of the filtrate and realizes the recycling of resources.
[0032] (2) When the carbonization starting temperature is less than 30°C, the present invention can obtain relatively large cubic nano-calcium carbonate, and the size is mostly concentrated between 100-200 nanometers.
[0033] (3) In the present invention, when the carbonization starting temperature is greater than 30°C, rod-shaped nano calcium carbonate with a length of several hundred nanometers can be obtained.
[0034] (4) The method of the present invention is extremely simple and suitable for industrial large-scale production, and can produce cubic nano calcium carbonate and rod-shaped nano calcium carbonate with good dispersion and a size distribution of 80-200 nm without adding a crystal control agent. It has broad industrial application prospects and market prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a morphology diagram of the product obtained in Example 1 of the present invention;
[0036] Figure 2 This is a morphology diagram of the product obtained in Example 2 of the present invention;
[0037] Figure 3 This is a morphology diagram of the product obtained in Example 3 of the present invention;
[0038] Figure 4 is a morphology diagram of the product obtained in Example 4 of the present invention;
[0039] Figure 5 This is a morphology diagram of the product obtained in Example 5 of the present invention;
[0040] Figure 6 This is a morphology diagram of the product obtained in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0041] The technical solution of the present invention is further described in detail below through specific embodiments in conjunction with the accompanying drawings.
[0042] The invention provides a method for preparing nano calcium carbonate. The method comprises the following steps: digesting a substance containing calcium oxide to obtain lime milk, subjecting the lime milk to carbonization reaction with a gas containing carbon dioxide after aging, and obtaining nano calcium carbonate after treatment, wherein a soluble salt is further added during the reaction.
[0043] In the present invention, the content of calcium oxide in the substance containing calcium oxide is not less than 90%; more preferably, the substance containing calcium oxide is quicklime or calcium oxide, wherein the quicklime can be obtained by calcining and decomposing limestone.
[0044] In the present invention, the soluble salt is added at any time point before the carbonization reaction of the preparation method; for example, the soluble salt is added during digestion, or after digestion is completed, or before the carbonization reaction. More preferably, the soluble salt is added as follows:
[0045] a. dissolving a soluble salt in water to obtain a soluble salt solution, digesting the substance containing calcium oxide with the soluble salt solution, and performing subsequent steps;
[0046] or b. digesting the substance containing calcium oxide and water to obtain lime milk, adding a soluble salt to the lime milk and dissolving it, and performing subsequent steps;
[0047] or c. digesting the substance containing calcium oxide and water to obtain lime milk and aging it, adding a soluble salt to the aged lime milk and dissolving it, and then carrying out the subsequent steps.
[0048] In the present invention, the soluble salt is a soluble sodium salt or a soluble potassium salt, and more preferably the soluble salt is at least one of sodium chloride, sodium sulfate, sodium nitrate, sodium phosphate, and sodium hexametaphosphate. By adopting the technical solution, the selection of a soluble sodium salt can further reduce costs while achieving the technical effect.
[0049] In the present invention, the ratio of the total amount of the soluble salt added to the amount of calcium oxide in the substance containing calcium oxide is between 0.5-4:1, preferably between 1-3:1, and most preferably between 1.5-2:1.
[0050] In the present invention, the water temperature during digestion is controlled at 30-80° C., preferably 40-70° C., and most preferably 50-60° C. This can further ensure that calcium oxide fully reacts with water and reduce interference with the product in the later stage.
[0051] In the present invention, the mass ratio of the digestion water to the calcium oxide in the substance containing calcium oxide is between 4:1-6:1, but before the carbonization reaction, the concentration of calcium hydroxide in the lime milk is adjusted to be no higher than 1.5 mol / L, and the more preferred concentration of calcium hydroxide is between 0.8 and 1.5 mol / L. It can further ensure that the viscosity of the reaction system will not be too large, avoiding a significant impact on the morphology of the product; at the same time, considering the economic cost factor, it is more suitable to be in the range of 0.8 to 1.5 mol / L, which can be selected and fine-tuned according to the actual production working conditions.
[0052] In the present invention, the dosage of the gas containing carbon dioxide is calculated based on the ratio of the minute ventilation volume (L / min) of carbon dioxide to the amount of calcium oxide in the substance containing calcium oxide of 0.1 to 1:1.
[0053] In the present invention, the carbonization reaction temperature is 5-30°C, which can obtain cubic nano-calcium carbonate with good dispersibility, more preferably 10-25°C, more preferably 15-20°C. Under the preferred temperature range, purer cubic nano-calcium carbonate can be obtained, and the presence of rod-shaped nano-calcium carbonate can be reduced.
[0054] In the present invention, the carbonization reaction temperature is 30-60°C, which can obtain rod-shaped nano-calcium carbonate with good dispersibility, preferably 35-55°C, and most preferably 40-50°C. In the preferred temperature range, purer rod-shaped nano-calcium carbonate can be obtained, and the presence of cubic nano-calcium carbonate can be reduced.
[0055] In the present invention, the treatment includes surface treatment, and the surface treatment is surface coating treatment using a coating agent. More preferably, the coating agent is a conventional coating agent such as sodium stearate. More preferably, the amount of the coating agent is 3-4% of the mass of calcium carbonate. More preferably, the surface treatment is carried out at 70-85°C.
[0056] In the present invention, the treatment also includes conventional treatment steps such as filtration, washing, and drying.
[0057] In the present invention, the preparation method can also use limestone as raw material, calcine and decompose it into quicklime calcium oxide, then digest and age it, and then introduce gas containing carbon dioxide to carry out carbonization reaction. When the solution pH is 7, continue to aerate for 15 minutes and then stop aeration. After surface treatment, filtering, washing and drying, nano calcium carbonate is obtained; soluble salt is also added during the reaction process.
[0058] In the present invention, the preparation method specifically comprises the following steps:
[0059] 1) water at a certain temperature and a substance containing calcium oxide are subjected to a digestion reaction in a certain ratio to obtain lime milk;
[0060] 2) Add a certain amount of soluble salts to the lime milk;
[0061] 3) After aging the lime milk for 24 hours, filtering and removing slag, introducing carbon dioxide or kiln gas containing carbon dioxide into the obtained refined lime milk for carbonization reaction;
[0062] 4) When the solution pH = 7, continue to ventilate for 15 minutes, then stop ventilating, raise the temperature to 70-85°C, and add sodium stearate coating agent for surface coating treatment;
[0063] 5) The coated calcium carbonate is filtered, washed three times and then dried to obtain nano calcium carbonate.
[0064] The scheme of the present invention is further described below with reference to specific examples and drawings.
[0065] Example 1
[0066] Step 1: Put the calcium carbonate raw material crushed to a size of 4-8 cm into a muffle furnace and calcine at 1000°C.
[0067] Step 2: Take 112g of calcined calcium oxide, add it into 560g of water, the water temperature is 60℃, stir vigorously for 3h, age it for 24h after digestion, and then sieve it through a 200-mesh sieve to remove the residue (if there is no residue, sieving is not required).
[0068] Step 3: Add 234g NaCl and stir to dissolve.
[0069] Step 4: add water to adjust the concentration of calcium hydroxide in the lime milk to 0.94 mol / L, control the temperature of the lime milk to 25°C, and introduce a mixed gas of carbon dioxide and air at a ventilation rate of 2 L / min; wherein the ventilation rate of carbon dioxide is 0.3 L / min, and the concentration of carbon dioxide is 15%.
[0070] Step 5: When the solution pH = 7, continue to ventilate for 15 minutes and then stop ventilating, raise the temperature to 85° C., add sodium stearate coating agent for surface coating treatment, and the amount of sodium stearate used is 3% of the mass of nano-calcium carbonate.
[0071] Step 6: Filter the product of step 5, wash it three times and then dry it to obtain cubic nano calcium carbonate with a particle size range of 80 to 200 nm. Figure 1 .
[0072] Example 2
[0073] Step 1: Place the crushed, ground and screened calcium carbonate raw materials into a muffle furnace and calcine at 1000°C.
[0074] Step 2: Take 168g of calcined calcium oxide, add it to 672g of water, the water temperature is 50°C, stir vigorously for 3h, age it for 24h after digestion, and then filter and remove the slag.
[0075] Step 3: Add 175.5g sodium chloride and 51g sodium nitrate and stir to dissolve.
[0076] Step 4: add water to adjust the concentration of calcium hydroxide in the lime milk to 1.45 mol / L, control the temperature of the lime milk to 40°C, introduce a mixed gas of carbon dioxide and air, the carbon dioxide ventilation rate is 0.3 L / min, and the concentration of carbon dioxide is 30%.
[0077] Step 5: When the solution pH = 7, continue to ventilate for 15 minutes and then stop ventilating, raise the temperature to 80° C., add sodium stearate coating agent for surface coating treatment, and the amount of sodium stearate used is 4% of the mass of nano-calcium carbonate.
[0078] Step 6: Filter the product, wash it three times and then dry it to obtain calcium carbonate, such as Figure 2 .
[0079] Example 3
[0080] Step 1: Place the crushed, ground and screened calcium carbonate raw materials into a muffle furnace and calcine at 1000°C.
[0081] Step 2: Take 168g of calcined calcium oxide, add it to 672g of water, the water temperature is 50°C, stir vigorously for 3h, age it for 24h after digestion, and then filter and remove the slag.
[0082] Step 3: Add 351g of sodium chloride and stir to dissolve.
[0083] Step 4: add water to adjust the concentration of calcium hydroxide in the lime milk to 1.2 mol / L, control the temperature of the lime milk to 40°C, introduce a mixed gas of carbon dioxide and air, the carbon dioxide ventilation rate is 0.3 L / min, and the concentration of carbon dioxide is 20%.
[0084] Step 5: When the solution pH = 7, continue to ventilate for 15 minutes and then stop ventilating, raise the temperature to 80° C., add sodium stearate coating agent for surface coating treatment, and the amount of sodium stearate used is 3% of the mass of nano-calcium carbonate.
[0085] Step 6: Filter the product, wash it three times and then dry it to obtain calcium carbonate, such as Figure 3 , it can be seen that the obtained nano calcium carbonate is rod-shaped.
[0086] Example 4
[0087] The steps are the same as in Example 3, except that the carbonization starting temperature is adjusted from 40°C to 30°C. The obtained product is as follows Figure 4 , it can be seen that the obtained nano calcium carbonate has both rod-shaped and cubic shapes.
[0088] Example 5
[0089] The steps are the same as in Example 3, except that the carbonization starting temperature is adjusted from 40°C to 20°C. The obtained product is as follows Figure 5 , it can be seen that the obtained nano calcium carbonate is cubic.
[0090] Comparative Example 1
[0091] The steps are the same as in Example 1, except that the amount of sodium chloride added is 58.5 g. The obtained product is as follows Figure 6 From the comparison between this comparative example and Example 1, it can be seen that when the concentration of soluble salt is low, the particle size of the obtained calcium carbonate product is uncontrollable, the morphology is irregular, and a large amount of agglomeration is obtained; however, after adding high concentration salt, a cubic nano calcium carbonate with a regular morphology and a particle size range of 80 to 200 nm can be obtained, and it has excellent dispersibility.
[0092] The above-described embodiments are only preferred solutions of the present invention and are not intended to limit the present invention in any form. Other variations and modifications are possible without exceeding the technical solutions described in the claims.
Claims
1. A method for preparing nano calcium carbonate, characterized in that, The preparation method comprises the following steps: digesting a substance containing calcium oxide to obtain lime milk, and then subjecting the lime milk to carbonization reaction with gas containing carbon dioxide after aging, and obtaining nano calcium carbonate after treatment, wherein soluble salt is also added in the process; the soluble salt is at least one of soluble sodium salt, soluble potassium salt and soluble lithium salt, and the ratio of the total amount of the soluble salt added to the amount of calcium oxide in the substance containing calcium oxide is 0.5-4:1; the mass ratio of water in the digestion to calcium oxide in the substance containing calcium oxide is 4-6:1, and before the carbonization reaction, the concentration of calcium hydroxide in the lime milk is adjusted to be not higher than 1.5 mol / L; the carbonization reaction temperature is 30-60°C, and rod-shaped nano calcium carbonate is obtained.
2. A method for preparing nano calcium carbonate according to claim 1, characterized in that: The content of calcium oxide in the substance containing calcium oxide is not less than 90%.
3. A method for preparing nano calcium carbonate according to claim 1, characterized in that: The soluble salt is added at any time point before the carbonization reaction of the preparation method.
4. A method for preparing nano calcium carbonate according to claim 1, characterized in that: The soluble salt is added during digestion, or after digestion is completed, or before carbonization reaction.
5. A method for preparing nano calcium carbonate according to claim 1, characterized in that: The preparation method specifically comprises the following steps: 1) subjecting water to a digestion reaction with a substance containing calcium oxide to obtain lime milk; 2) adding soluble salt to the lime milk; 3) aging the lime milk for 24 hours, filtering and removing slag, and introducing carbon dioxide or kiln gas containing carbon dioxide into the obtained refined lime milk for carbonization reaction; 4) When the solution pH = 7, continue to ventilate for 15 minutes, then stop ventilating, raise the temperature to 70-85°C, and add a coating agent for surface coating treatment; 5) The coated calcium carbonate is filtered, washed and dried to obtain nano calcium carbonate.