Acid-alkali resistant floor material and preparation method thereof

The acid-alkali-resistant floor materials prepared by using activated calcium carbonate powder, calcined basalt powder, pyrote sand, silicon fume and boron nitride micropowder are solved by solving the high cost, complex construction and use of traditional vinyl resin floor materials. The problem of short life span achieves low cost, high durability and environmentally friendly floor anti-corrosion effects.

CN116477859BActive Publication Date: 2024-11-26HEBEI ZICHEN ARCHITECTURAL DECORATION ENG CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310425809.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-11-26
Estimated Expiration
2043-04-19

AI Technical Summary

Technical Problem

Traditional vinyl resin floor materials have high cost, complex construction, short service life, and are harmful to the human body and the environment, so they cannot effectively protect the corrosion of the floor from acid and alkaline media.

Method used

The acid-alkali floor materials are prepared by raw materials such as activated calcium carbonate powder, calcined basalt powder, pyrote sand, silicon fume and boron nitride micro powder. They are made by stirring evenly and sprinkling and grinding, which has good acid-alkali resistance and alkali resistance. Durability.

Benefits of technology

It reduces the cost of floor anti-corrosion materials, extends service life, improves the simplicity of construction and durability of floors, reduces oil imports, and provides effective protection against acid and alkaline media.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to the field of floor materials, and in particular to an acid- and alkali-resistant floor material and a preparation method thereof. The acid- and alkali-resistant floor material is composed of the following raw materials: 4-6 parts of activated calcium carbonate powder, 25-35 parts of calcined basalt powder, 55-65 parts of pyrite sand, 2-4 parts of silica ash, 8-12 parts of boron nitride powder, and 4-6 parts of white carbon black. The acid- and alkali-resistant floor material has low raw material cost, long service life, and simple construction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of floor materials, and in particular to an acid- and alkali-resistant floor material and a preparation method thereof. Background Art

[0002] With the rapid development of my country's industry, the anti-corrosion of industrial plant floors is becoming more and more important. The traditional floor anti-corrosion in the market is still dominated by vinyl anti-corrosion floors. Paint anti-corrosion floors are mainly based on vinyl resins, which are two-component coatings. They began to be domestically produced in 1975. Vinyl resins have been used for ground anti-corrosion at home and abroad. Vinyl resin anti-corrosion floors are used to overcome the problem of acid and alkali resistance. Vinyl resin (plastic) is a synthetic resin extracted from petroleum, which consumes a lot of petroleum. However, my country is a country with scarce petroleum resources. At the same time, the construction process of vinyl resin anti-corrosion floors (three cloths and five oils) is complex, the material cost is high, and the general market price is more than 100 yuan / ㎡.

[0003] The service life of vinyl resin anti-corrosion flooring is 10-15 years. Long-term contact with human body will cause dry, cracked and rough skin. The free aromatic hydrocarbons and plasticizers it contains will cause certain toxicity to the human liver, kidneys and hematopoietic system. It is also not fireproof, water-resistant, or high-temperature resistant, and is prone to volatile toxic substances. It is a Class III dangerous good and a flammable liquid.

[0004] Anticorrosive mortars usually include: cationic chloroprene cement mortar (two-component), acrylic mortar (two-component), epoxy mortar (two-component), polyurethane mortar (two-component), and aluminate anticorrosive mortar (single component). Since chloroprene cement mortar, acrylic mortar, epoxy mortar, and polyurethane mortar are all two-component and must be mixed with various anticorrosive emulsions and mortars before use, they can only be used for wall anticorrosion masonry and plastering, and cannot be used with water. Aluminate anticorrosive mortars with water can only withstand concentrations less than 1 It cannot be used in acidic media with an acid content of less than 0%. It cannot be used in acidic media with an acid content of more than 10% after adding water. Aluminate anti-corrosion mortar is mainly composed of water glass and high-alumina cement, which is a weakly alkaline cement mainly composed of calcium aluminate, which is soluble in acid. Therefore, it cannot maintain its strength for a long time and can only withstand mild corrosion. It has poor weather resistance and its service life is 3-4 years before it needs to be replaced again. Therefore, anti-corrosion mortar has not been a good solution to the floor anti-corrosion technology. Due to technical defects, it has not been widely promoted and used in the market. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art, avoid the high cost of raw materials, large pollution and complicated construction of traditional acid-alkali resistant floor, and provide an acid-alkali resistant floor material and a preparation method thereof. The present invention has low raw material cost, long service life and simple construction.

[0006] The object of the present invention is achieved through the following measures: an acid and alkali resistant floor material, composed of the following raw materials: 4-6 parts of activated calcium carbonate powder, 25-35 parts of calcined basalt powder, 55-65 parts of pyrite sand, 2-4 parts of silica ash, 8-12 parts of boron nitride powder, and 4-6 parts of white carbon black.

[0007] The above-mentioned acid- and alkali-resistant floor material is composed of the following raw materials: 5 parts of activated calcium carbonate powder, 30 parts of calcined basalt powder, 60 parts of pyrite sand, 3 parts of silica ash, 10 parts of boron nitride powder, and 5 parts of white carbon black.

[0008] In the above-mentioned acid- and alkali-resistant floor material, the particle size of the activated calcium carbonate powder is 325 mesh.

[0009] In the above-mentioned acid- and alkali-resistant floor material, the particle size of the calcined basalt powder is 325 mesh.

[0010] The above-mentioned acid- and alkali-resistant floor material, the particle size of the pyrite sand is 8-30 mesh.

[0011] The above-mentioned acid- and alkali-resistant floor material, the sulfur content of the pyrite sand is ≥50%.

[0012] The preparation method of the above-mentioned acid-alkali resistant floor material comprises the following steps:

[0013] S1: Prepare raw materials, weigh 4-6 parts of activated calcium carbonate powder, 25-35 parts of calcined basalt powder, 55-65 parts of pyrite sand, 2-4 parts of silica fume, 8-12 parts of boron nitride powder, and 4-6 parts of white carbon black, and set aside;

[0014] S2: Mixing: Put the activated calcium carbonate powder, calcined basalt powder, pyrite sand, silica fume, boron nitride powder and white carbon black prepared in S1 into a mixer, mix well to obtain the finished product.

[0015] Calcium carbonate is an inorganic compound with the chemical formula CaCO3. It is the main component of limestone, marble, etc. It is usually white crystals and odorless. After modification, calcium carbonate is basically insoluble in water and does not react with acids and alkalis.

[0016] Basalt is a basic volcanic rock, its main component is silicon dioxide, it has strong chemical corrosion resistance, excellent performance, stable structure, stable performance, acid and alkali corrosion resistance, good durability, and can improve the floor's crack resistance, stability and corrosion resistance. After calcination modification, basalt has higher purity and more stable acid and alkali corrosion resistance.

[0017] Pyrite sand, as the main aggregate in the present invention, has a sulfur content of more than 50%. Pyrite sand is an important raw material for extracting sulfuric acid. Experiments have shown that it has strong acid resistance. At the same time, mixed grading with different mesh sizes and a combination of coarse and fine can make the floor more compact. Pyrite sand is concentrated in South China, North China, and Southwest China, with large reserves and easy procurement.

[0018] Silica fume is used as an auxiliary cementitious material to increase the bonding force of powder. The powder here replaces cement, which refers to the calcined basalt powder, boron nitride powder, and activated calcium carbonate powder in the raw materials. Silica fume is the smoke that escapes with the exhaust gas during the high-temperature smelting of industrial silicon and ferrosilicon in industrial electric furnaces and is treated by a special collection device. The SiO2 content accounts for 90% of the total smoke. The particles are very small, and the average particle size is almost nanometer-level. Silica fume is not easy to react with other substances, and does not react chemically with most acids and alkalis. Its particles evenly cover the surface of the object and have strong corrosion resistance.

[0019] Boron nitride micropowder has strong resistance to chemical corrosion, is not corroded by inorganic acids, is resistant to high temperatures (up to about 1700 degrees), heat-resistant alkalis, and has high hardness, which further improves the acid and alkali resistance of the entire powder and increases the hardness of the floor.

[0020] White carbon black is a general term for white powdered X-ray amorphous silicic acid and silicate products, mainly precipitated silica, fumed silica and ultrafine silica gel, and also includes powdered synthetic aluminum silicate and calcium silicate. White carbon black is a porous substance, and its composition can be expressed by SiO2·nH2O, where nH2O exists in the form of surface hydroxyl groups. It is resistant to high temperatures, non-flammable, tasteless, odorless, and has good electrical insulation. Tests have shown that it has strong corrosion resistance.

[0021] The mixture of calcined basalt powder, boron nitride powder, activated calcium carbonate powder and silica fume can improve the bonding strength of the entire raw material and replace cement. Because almost all cements such as traditional silicate water, aluminate, slag cement, volcanic ash water, fly ash composite cement, etc. will react with acid and alkali, resulting in poor acid and alkali resistance of the floor.

[0022] The acid-alkali resistant floor of the present invention is an inorganic material, which is non-toxic and tasteless, and is simple and convenient to construct. When the concrete is initially set, the material is spread by a spreading machine or manually (in two times) with a thickness of 1.5 cm, and then it can be ground, compacted and polished by a driving trowel. The Mohs hardness reaches level 7, and it is strong and durable.

[0023] Beneficial effects of the invention: The invention focuses on solving the problems of complex construction technology, high material cost, and short service life of the existing vinyl anti-corrosion floor. It can be rolled over by forklifts and heavy trucks for a long time, making the ground resistant to heavy corrosion, strong acid and alkali, reducing the investment cost and maintenance cost of the enterprise, increasing the service life of the floor, and also reducing the amount of oil imports. It has been verified that the cost of the acid and alkali resistant floor of the invention is 60 yuan / ㎡, including labor and materials, which greatly reduces the cost of floor anti-corrosion, and the service life is almost synchronized with the life of concrete. DETAILED DESCRIPTION

[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Example 1: An acid- and alkali-resistant floor material is composed of the following raw materials: 4 Kg of activated calcium carbonate powder, 25 Kg of calcined basalt powder, 55 Kg of pyrite sand, 2 Kg of silica ash, 8 Kg of boron nitride powder, and 4 Kg of white carbon black.

[0026] In the above-mentioned acid- and alkali-resistant floor material, the particle size of the activated calcium carbonate powder is 325 mesh.

[0027] In the above-mentioned acid- and alkali-resistant floor material, the particle size of the calcined basalt powder is 325 mesh.

[0028] The above-mentioned acid- and alkali-resistant floor material, the particle size of the pyrite sand is 8 mesh.

[0029] The above-mentioned acid- and alkali-resistant floor material, the sulfur content of the pyrite sand is ≥50%.

[0030] The preparation method of the above-mentioned acid-alkali resistant floor material comprises the following steps:

[0031] S1: Prepare raw materials, weigh 4 kg of activated calcium carbonate powder, 25 kg of calcined basalt powder, 55 kg of pyrite sand, 2 kg of silica fume, 8 kg of boron nitride powder, and 4 kg of white carbon black, and set aside;

[0032] S2: Mixing: Put the activated calcium carbonate powder, calcined basalt powder, pyrite sand, silica fume, boron nitride powder and white carbon black prepared in S1 into a mixer, mix well to obtain the finished product.

[0033] Example 2: An acid- and alkali-resistant floor material, composed of the following raw materials: 6 Kg of activated calcium carbonate powder, 35 Kg of calcined basalt powder, 65 Kg of pyrite sand, 4 Kg of silica ash, 12 Kg of boron nitride powder, and 6 Kg of white carbon black.

[0034] In the above-mentioned acid- and alkali-resistant floor material, the particle size of the activated calcium carbonate powder is 325 mesh.

[0035] In the above-mentioned acid- and alkali-resistant floor material, the particle size of the calcined basalt powder is 325 mesh.

[0036] The above-mentioned acid- and alkali-resistant floor material, the particle size of the pyrite sand is 30 mesh.

[0037] The above-mentioned acid- and alkali-resistant floor material, the sulfur content of the pyrite sand is ≥50%.

[0038] The preparation method of the above-mentioned acid-alkali resistant floor material comprises the following steps:

[0039] S1: Prepare raw materials, weigh 6 kg of activated calcium carbonate powder, 35 kg of calcined basalt powder, 65 kg of pyrite sand, 4 kg of silica fume, 12 kg of boron nitride powder, and 6 kg of white carbon black, and set aside;

[0040] S2: Mixing: Put the activated calcium carbonate powder, calcined basalt powder, pyrite sand, silica fume, boron nitride powder and white carbon black prepared in S1 into a mixer, mix well to obtain the finished product.

[0041] Example 3: An acid- and alkali-resistant floor material is composed of the following raw materials: 5 Kg of activated calcium carbonate powder, 30 Kg of calcined basalt powder, 60 Kg of pyrite sand, 3 Kg of silica ash, 10 Kg of boron nitride powder, and 5 Kg of white carbon black.

[0042] In the above-mentioned acid- and alkali-resistant floor material, the particle size of the activated calcium carbonate powder is 325 mesh.

[0043] In the above-mentioned acid- and alkali-resistant floor material, the particle size of the calcined basalt powder is 325 mesh.

[0044] The above-mentioned acid- and alkali-resistant floor material, the particle size of the pyrite sand is 19 mesh.

[0045] The above-mentioned acid- and alkali-resistant floor material, the sulfur content of the pyrite sand is ≥50%.

[0046] The preparation method of the above-mentioned acid-alkali resistant floor material comprises the following steps:

[0047] S1: Prepare raw materials, weigh 5 kg of activated calcium carbonate powder, 30 kg of calcined basalt powder, 60 kg of pyrite sand, 3 kg of silica fume, 10 kg of boron nitride powder, and 5 kg of white carbon black, and set aside;

[0048] S2: Mixing: Put the activated calcium carbonate powder, calcined basalt powder, pyrite sand, silica fume, boron nitride powder and white carbon black prepared in S1 into a mixer, mix well to obtain the finished product.

[0049] Example 4: An acid- and alkali-resistant floor material is composed of the following raw materials: 4 Kg of activated calcium carbonate powder, 35 Kg of calcined basalt powder, 57 Kg of pyrite sand, 3 Kg of silica ash, 12 Kg of boron nitride powder, and 4 Kg of white carbon black.

[0050] In the above-mentioned acid- and alkali-resistant floor material, the particle size of the activated calcium carbonate powder is 325 mesh.

[0051] In the above-mentioned acid- and alkali-resistant floor material, the particle size of the calcined basalt powder is 325 mesh.

[0052] The above-mentioned acid- and alkali-resistant floor material, the particle size of the pyrite sand is 30 mesh.

[0053] The above-mentioned acid- and alkali-resistant floor material, the sulfur content of the pyrite sand is ≥50%.

[0054] The preparation method of the above-mentioned acid-alkali resistant floor material comprises the following steps:

[0055] S1: Prepare raw materials, weigh 4 kg of activated calcium carbonate powder, 35 kg of calcined basalt powder, 57 kg of pyrite sand, 3 kg of silica fume, 12 kg of boron nitride powder, and 4 kg of white carbon black, and set aside;

[0056] S2: Mixing: Put the activated calcium carbonate powder, calcined basalt powder, pyrite sand, silica fume, boron nitride powder and white carbon black prepared in S1 into a mixer, mix well to obtain the finished product.

[0057] Example 5: An acid- and alkali-resistant floor material, composed of the following raw materials: 6 Kg of activated calcium carbonate powder, 30 Kg of calcined basalt powder, 63 Kg of pyrite sand, 3 Kg of silica ash, 8 Kg of boron nitride powder, and 6 Kg of white carbon black.

[0058] In the above-mentioned acid- and alkali-resistant floor material, the particle size of the activated calcium carbonate powder is 325 mesh.

[0059] In the above-mentioned acid- and alkali-resistant floor material, the particle size of the calcined basalt powder is 325 mesh.

[0060] The above-mentioned acid- and alkali-resistant floor material, the particle size of the pyrite sand is 28 mesh.

[0061] The above-mentioned acid- and alkali-resistant floor material, the sulfur content of the pyrite sand is ≥50%.

[0062] The preparation method of the above-mentioned acid-alkali resistant floor material comprises the following steps:

[0063] S1: Prepare raw materials, weigh 6 kg of activated calcium carbonate powder, 30 kg of calcined basalt powder, 63 kg of pyrite sand, 3 kg of silica fume, 8 kg of boron nitride powder, and 6 kg of white carbon black, and set aside;

[0064] S2: Mixing: Put the activated calcium carbonate powder, calcined basalt powder, pyrite sand, silica fume, boron nitride powder and white carbon black prepared in S1 into a mixer, mix well to obtain the finished product.

[0065] Example 6: An acid- and alkali-resistant floor material, composed of the following raw materials: 5 Kg of activated calcium carbonate powder, 35 Kg of calcined basalt powder, 58 Kg of pyrite sand, 2 Kg of silica ash, 10 Kg of boron nitride powder, and 5 Kg of white carbon black.

[0066] In the above-mentioned acid- and alkali-resistant floor material, the particle size of the activated calcium carbonate powder is 325 mesh.

[0067] In the above-mentioned acid- and alkali-resistant floor material, the particle size of the calcined basalt powder is 325 mesh.

[0068] The above-mentioned acid- and alkali-resistant floor material, the particle size of the pyrite sand is 10 mesh.

[0069] The above-mentioned acid- and alkali-resistant floor material, the sulfur content of the pyrite sand is ≥50%.

[0070] The preparation method of the above-mentioned acid-alkali resistant floor material comprises the following steps:

[0071] S1: Prepare raw materials, weigh 5 kg of activated calcium carbonate powder, 35 kg of calcined basalt powder, 58 kg of pyrite sand, 2 kg of silica fume, 10 kg of boron nitride powder, and 5 kg of white carbon black, and set aside;

[0072] S2: Mixing: Put the activated calcium carbonate powder, calcined basalt powder, pyrite sand, silica fume, boron nitride powder and white carbon black prepared in S1 into a mixer, mix well to obtain the finished product.

[0073] The following table compares the performance of the vinyl heavy-duty anti-corrosion floor on the market and the acid-alkali resistant floor of the present invention:

[0074]

[0075] The following table shows the performance tests performed on the products of the present invention:

[0076]

[0077]

[0078] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An acid and alkali resistant floor material, characterized by: The invention is composed of the following raw materials: 4-6 parts of activated calcium carbonate powder, 25-35 parts of calcined basalt powder, 55-65 parts of pyrite sand, 2-4 parts of silica fume, 8-12 parts of boron nitride powder and 4-6 parts of white carbon black.

2. The acid- and alkali-resistant floor material according to claim 1, characterized in that: It is composed of the following raw materials: 5 parts of activated calcium carbonate powder, 30 parts of calcined basalt powder, 60 parts of pyrite sand, 3 parts of silica fume, 10 parts of boron nitride powder and 5 parts of white carbon black.

3. An acid-alkali resistant floor material according to claim 1 or 2, characterized in that: The particle size of the activated calcium carbonate powder is 325 meshes.

4. The acid-alkali resistant floor material according to claim 1 or 2, characterized in that: The particle size of the calcined basalt powder is 325 mesh.

5. The acid-alkali resistant floor material according to claim 1 or 2, characterized in that: The particle size of the pyrite sand is 8-30 meshes.

6. The acid-alkali resistant floor material according to claim 5, characterized in that: The sulfur content of the pyrite sand is ≥50%.

7. A method for preparing the acid-alkali resistant floor material according to claim 1, characterized in that: The steps include: S1: Prepare raw materials, weigh 4-6 parts of activated calcium carbonate powder, 25-35 parts of calcined basalt powder, 55-65 parts of pyrite sand, 2-4 parts of silica fume, 8-12 parts of boron nitride powder, and 4-6 parts of white carbon black, and set aside; S2: Mixing: Put the activated calcium carbonate powder, calcined basalt powder, pyrite sand, silica fume, boron nitride powder and white carbon black prepared in S1 into a mixer, mix well to obtain the finished product.

Citation Information

Patent Citations

  • Preparation method of high-wear-resistance floor paint

    CN106519879A

  • Carborundum floor material and application thereof

    CN114292065A

  • Extra quick hardening and high flowable mortar composition, and extra quick hardening and high flowable mortar

    JP2005162508A