Active composite powder based on steel slag and slag and preparation method thereof
The active composite powder prepared by mixing steel slag, slag and other components in specific proportions and adding active activators solves the problem of low activity of iron and steel metallurgical solid waste, achieves high hydration activity and resource utilization, and improves the performance of cement concrete. performance and environmental performance.
Patent Information
- Application Number
- CN202310407537.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-04-17
AI Technical Summary
The activity of iron and steel metallurgical solid wastes such as steel slag, steel tailings mud and mine tailings mud is low, resulting in unsatisfactory application results in cement concrete materials, and failure to effectively utilize resources, resulting in environmental pollution and resource waste.
Develop an active composite powder based on steel slag and slag. By mixing steel slag powder, slag powder, steel tailings powder mud and mine tailings powder mud in specific proportions, and adding an active activator, such as maleic acid monomer. Active composite powders with high hydration activity are prepared by grinding triisopropanolamine ester sulfonate, N-dodecylethanolamine, etc.
Significantly improves the hydration activity of the composite powder, realizes the resource utilization of solid wastes such as steel slag, steel tailings mud, and mine tailings mud, solves the problems of solid waste accumulation and insufficient auxiliary cementitious materials, and improves the performance of cement concrete. performance and environmental performance.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of building materials, and in particular to an active composite powder based on steel slag and slag and a preparation method thereof. Background Art
[0002] As a key industry for carbon emissions and material and energy consumption, the cement concrete industry will be the main area for promoting national energy conservation and emission reduction. The development of green and low-carbon cement concrete materials is imperative. Using industrial by-products with potential hydraulic activity to prepare cement concrete materials can not only reduce the amount of cement used, reduce cement clinker production, and be beneficial to energy conservation and emission reduction, but also make solid wastes be recycled, and promote the green, low-carbon and sustainable development of the cement concrete industry.
[0003] The iron and steel metallurgical industry generates a large amount of industrial solid waste every year. At present, except for slag which is widely used as an auxiliary cementitious material in cement concrete, other iron and steel metallurgical solid wastes have not been effectively utilized as resources. For example, steel slag. my country discharges about 100 million tons of steel slag every year, but its utilization rate is low, with a comprehensive utilization rate of less than 30%, resulting in a large amount of steel slag in a state of accumulation, which not only occupies land but also pollutes the environment. In addition, the steel tailings mud generated in the process of magnetic separation of steel slag to recover iron, and the mine tailings mud generated in the process of iron ore beneficiation, have huge emissions and are difficult to utilize, and are difficult to treat solid wastes. Therefore, it is urgent to improve and promote the technical level of resource utilization of difficult-to-treat solid wastes in the steel industry.
[0004] From the perspective of chemical and mineral composition, steel slag and cement clinker are very similar, and there is great potential for their application in cement concrete materials. At the same time, with the improvement of steel slag treatment technology this year, undesirable components in steel slag, such as dead burnt lime and composition fluctuations, have been controlled and improved to a great extent, thus providing a quality basis for the grinding of steel slag and the use of steel slag powder in cement concrete materials. However, due to the low hydration activity of steel slag itself, the effect of using it alone as an auxiliary cementitious material in cement concrete is not ideal. In addition, although solid wastes such as steel tailings mud and mine tailings mud contain more or less cementitious minerals, most of them are in a dumping state due to their low activity and poor performance, and have not been able to achieve resource utilization of building materials. Therefore, there is an urgent need for breakthroughs in the activity enhancement technology of solid wastes such as steel slag, steel tailings mud, and mine tailings mud. Summary of the invention
[0005] To this end, an embodiment of the present application provides an active composite powder based on steel slag and mineral slag, which aims to improve the resource utilization of solid wastes such as steel slag, steel tailings mud, and mine tailings mud, effectively improves the hydration activity of the composite powder, and can be promoted and applied in different types of cement concrete.
[0006] In a first aspect, the present application provides an active composite powder based on steel slag or slag, wherein the active composite powder comprises the following components in parts by mass:
[0007] 20-50 parts of steel slag powder, 40-70 parts of slag powder, 5-15 parts of steel tailings powder mud, 0-10 parts of mine tailings powder mud and 0-0.2 parts of active activator;
[0008] The active stimulant is composed of 2 to 15 parts of triisopropanolamine maleate sulfonate, 0 to 15 parts of N-dodecylethanolamine, 5 to 15 parts of N,N-dimethylisopropanolamine, 0 to 1 part of propylene glycol polyoxypropylene ether, 10 to 20 parts of sodium thiosulfate and 40 to 70 parts of water.
[0009] In a preferred example of the present application, it can be further configured that the specific surface area of the steel slag powder is 430 to 600 m 2 / kg, and the particle size is less than 60μm; the components of the steel slag powder include dicalcium silicate, tricalcium silicate, tricalcium aluminate, dodecalycium heptaaluminate, calcium oxide and magnesium oxide minerals.
[0010] In a preferred example of the present application, it can be further configured that the specific surface area of the slag powder is 430 to 600 m 2 / kg, and the particle size is less than 60μm; the slag powder contains active alumina and / or silicon dioxide amorphous glass minerals.
[0011] In a preferred example of the present application, it can be further set that the specific surface area of the steel tailings sludge is 450-550m 2 / kg, and the particle size is less than 45μm; the steel tailings powder mud contains calcium oxide, silicon dioxide, ferric oxide, tricalcium silicate, dicalcium silicate, calcium ferrite and hydrated calcium silicate.
[0012] In a preferred example of the present application, it can be further set that the specific surface area of the mine tailings powder is 450-550m 2 / kg, and the particle size is less than 45μm; the mine tailings powder contains silicon dioxide and ferric oxide.
[0013] In a preferred example of the present application, it can be further configured that the specific surface area of the active composite powder is 450 to 550 m 2 / kg.
[0014] In a preferred example of the present application, it can be further configured that the 7d activity index of the active composite powder is not less than 60%.
[0015] In a preferred example of the present application, it can be further configured that the 28d activity index of the active composite powder is not less than 75%.
[0016] In a second aspect, the present application provides a method for preparing the active composite powder based on steel slag or slag provided in the first aspect, the preparation method comprising:
[0017] Step 1: pre-treating steel slag, ore slag, steel tailings mud, and mine tailings mud respectively to obtain steel slag powder, ore slag powder, steel tailings mud, and mine tailings mud;
[0018] Step 2: uniformly mixing 20 to 50 parts of steel slag powder, 40 to 70 parts of slag powder, 5 to 15 parts of steel tailings powder and 0 to 10 parts of mine tailings powder obtained after pretreatment to obtain a mixed solid powder;
[0019] Step 3: using a mixed solvent prepared from 2 to 15 parts of triisopropanolamine maleate sulfonate, 0 to 15 parts of N-dodecylethanolamine, 5 to 15 parts of N,N-dimethylisopropanolamine, 0 to 1 part of propylene glycol polyoxypropylene ether, 10 to 20 parts of sodium thiosulfate, and 40 to 70 parts of water as an active stimulant;
[0020] Step 4: Take 0-0.2 parts of active stimulant and spray or sprinkle evenly on the mixed solid powder, then transfer to the grinder and grind to a specific surface area of 450-550m 2 / kg, and the active composite powder is obtained.
[0021] To sum up, compared with the prior art, the beneficial effects brought about by the technical solution provided in the embodiments of the present application include at least the following: the present application makes full use of steel slag powder, steel tailings powder mud, and mine tailings powder mud, and combines slag powder and activity stimulant to develop an active composite powder that can replace slag powder and has higher activity, wherein the total amount of steel slag powder, steel tailings powder mud, and mine tailings powder mud can reach a maximum of more than 60%, which can effectively solve the accumulation problem of local steel slag, steel tailings mud, and mine tailings mud, and can also alleviate the problem of insufficient auxiliary cementitious materials such as slag powder in some areas.
[0022] The synergistic hydration effect between the components of the present invention can achieve the hydration super-additive effect of the active composite powder, making it have higher hydration activity and application effect; among them, some calcium heptaaluminate (C 12At the same time, the hydration of dicalcium silicate (C2S), tricalcium silicate (C3S) and free calcium oxide in the steel slag powder can also provide calcium hydroxide (Ca(OH)2) and alkalinity for the system, and promote the pozzolanic reaction of the slag powder. The pozzolanic reaction of the slag powder consumes the calcium hydroxide (Ca(OH)2) in the system, which in turn promotes the hydration reaction of C2S and C3S in the steel slag powder. On the other hand, C3S, C2S, calcium ferrite and hydrated calcium silicate exist in the steel tailings sludge, among which C3S and C2S can also participate in hydration, provide Ca(OH)2 and alkalinity for the system, and promote the pozzolanic reaction of the slag powder. In addition, the hydrated calcium silicate can provide hydrated calcium silicate crystal nucleus points for C3S and C2S silicate minerals in the steel slag and steel slag sludge, and promote the earliest hydration of silicate minerals. In addition, the mine tailings powder is mainly composed of SiO2 and Fe2O3, which plays a role of dispersion, dilution, filling and skeleton in the gelling system, which is conducive to the formation and accumulation of other gelling products. Therefore, the efficient synergistic hydration of each component promotes the super-superimposed hydration reaction of the active composite powder of the present application, making it have higher hydration activity and application effect.
[0023] The N,N-dimethylisopropanolamine and N-dodecylethanolamine components in the active stimulant of the present application can respectively complex the calcium ions in the silicate minerals and the aluminate minerals in the active composite powder, promote their early hydration or optimize the product; the triisopropanolamine monoester sulfonate of maleic acid can promote the further development of the later strength of the cementitious material made of the active composite powder; the propylene glycol polyoxypropylene ether component can eliminate the bubbles in the cementitious material made of the active composite powder, making the microstructure of the cementitious material more compact; sodium thiosulfate can promote the early strength of the cementitious material, and also has the function of adjusting the compatibility of the active composite powder with cement; in addition, the organic components in the active stimulant can improve the dispersibility of the active composite powder and prevent agglomeration.
[0024] Finally, the active stimulator of the present application generally has the function of improving the adaptability of the active composite powder of the present application in different cement concrete materials, and promoting its application effect in different types of cement-based materials, mine filling materials and other fields. DETAILED DESCRIPTION
[0025] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.
[0026] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application is clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0027] In addition, the term "and / or" in this application is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this application, unless otherwise specified, generally indicates that the associated objects before and after are in an "or" relationship.
[0028] The active composite powder based on steel slag and slag and the preparation method thereof provided in the present application are described in detail below.
[0029] The active composite powder based on steel slag and slag provided in the present application is first described. The active composite powder includes the following components in parts by weight:
[0030] 20-50 parts of steel slag powder, 40-70 parts of slag powder, 5-15 parts of steel tailings powder, 0-10 parts of mine tailings powder and 0-0.2 parts of active stimulant; the active stimulant is composed of triisopropanolamine monoester sulfonate, N-dodecylethanolamine, N,N-dimethylisopropanolamine, propylene glycol polyoxypropylene ether, sodium thiosulfate and water, wherein the mass fractions of each component are: 2-15 parts of triisopropanolamine monoester sulfonate, 0-15 parts of N-dodecylethanolamine, 5-15 parts of N,N-dimethylisopropanolamine, 0-1 part of propylene glycol polyoxypropylene ether, 10-20 parts of sodium thiosulfate, and 40-70 parts of water. The specific surface area of the active composite powder is 450-550m 2 / kg. Meanwhile, the 7d activity index of the active composite powder is not less than 60%, and the 28d activity index is not less than 75%.
[0031] The active composite powder of the present application makes the most of steel slag, steel tailings mud, and mine tailings mud, and combines slag and active stimulants to develop a low-carbon and environmentally friendly active composite powder that can replace slag powder without reducing activity. The total amount of steel slag, steel tailings mud, and mine tailings mud can reach a maximum of 60%. If it is promoted and used, it can effectively solve the accumulation problem of solid wastes such as steel slag, steel tailings mud, and mine tailings mud, and realize the resource recycling of solid wastes.
[0032] Specifically, steel slag powder is steel slag that has been crushed, magnetically separated, and pre-grinded to a specific surface area of 430-600m 2 / kg, and the particle size is less than 60μm. Controlling the specific surface area of the steel slag powder within the above range can make the cementitious material prepared from the composite powder containing the steel slag powder have a denser structure and improve stability.
[0033] The steel slag is selected from at least one of converter steel slag, electric furnace steel slag and ladle furnace steel slag used in the steel industry, wherein converter steel slag is steel slag discharged when using a converter to smelt steel, electric furnace steel slag is steel slag discharged when using an electric furnace to smelt steel, and ladle furnace steel slag is steel slag discharged when using a ladle furnace to smelt steel. The components of steel slag powder mainly include dicalcium silicate (C2S), tricalcium silicate (C3S), tricalcium aluminate (C3A), dodecaaluminate (C7aluminate), and calcium silicate (C8aluminate). 12 A7), calcium oxide (CaO) and magnesium oxide (MgO), and also contains small amounts of other oxides and sulfides, such as titanium dioxide (TiO2), vanadium pentoxide (V2O5), calcium sulfide and ferrous sulfide (FeS). Steel slag contains a large amount of dicalcium silicate (C2S) and tricalcium silicate (C3S), which give it good gelling properties.
[0034] Slag is granulated blast furnace slag, which is the industrial solid waste obtained after the molten material is quenched into granules during the smelting of pig iron in the blast furnace. The slag is crushed, magnetically separated, and pre-ground to a specific surface area of 430-600m 2 / kg, and the particle size is less than 60μm, which is used as slag powder for preparing active composite powder. The slag powder contains amorphous glass minerals of aluminum oxide and / or silicon dioxide, and also contains a small amount of dicalcium silicate, monocalcium silicate, etc.
[0035] Steel tailings sludge is a byproduct produced when steel companies use wet ball milling, magnetic separation and other processes to recover iron-containing substances in steel slag. It is then ground to a specific surface area of 450-550m 2 / kg, with a particle size of less than 45μm, as steel tailings sludge. Steel tailings sludge contains calcium oxide (CaO), silicon dioxide (SiO2), ferric oxide (Fe2O3), tricalcium silicate (C3S), dicalcium silicate (C2S), ferric acid (CaFe2O4) and hydrated calcium silicate.
[0036] Mine tailings are sludge byproducts produced during the beneficiation process of iron ore mines, and are ground to a specific surface area of 450-550m 2 / kg, and the fine powder with a particle size of less than 45μm is used as mine tailings mud. The main components of mine tailings mud are silicon dioxide (SiO2) and ferric oxide (Fe2O3), and there are also some magnesium oxide (MgO), calcium oxide (CaO), etc.
[0037] The active composite powder based on steel slag and slag provided in this application can replace part of cement clinker in cement production, or replace traditional mineral admixtures or auxiliary cementitious materials in concrete preparation, or be used as a full solid waste cementitious material in the preparation of mine filling materials. It has a wide range of applications and can realize the resource utilization of solid waste.
[0038] After the components of the active composite powder of the present application are mixed together, the components in each component can play a synergistic hydration effect and achieve a hydration super-additive effect. 12 A7) and tricalcium aluminate (C3A) can provide early gelling activity. At the same time, dicalcium silicate (C2S) and tricalcium silicate (C3S) in steel slag powder and free calcium oxide (CaO) can provide calcium hydroxide Ca(OH)2 and alkalinity to the system after hydration, thereby promoting the pozzolanic reaction in the slag powder without the need to add additional lime. The pozzolanic reaction refers to the reaction of active alumina and silicon dioxide in the slag powder with calcium hydroxide to generate reaction products such as hydrated calcium silicate and hydrated calcium aluminate. The pozzolanic reaction of the slag powder consumes Ca(OH)2 in the system, which in turn promotes the hydration reaction of dicalcium silicate (C2S) and tricalcium silicate (C3S) in the steel slag powder. On the other hand, there are tricalcium silicate (C3S), dicalcium silicate (C2S), ferric acid (CaFe2O4) and hydrated calcium silicate in steel tailings sludge. Among them, tricalcium silicate (C3S) and dicalcium silicate (C2S) can also participate in hydration, provide more Ca(OH)2 and alkalinity for the system, and promote the volcanic ash reaction of slag powder. Hydrated calcium silicate can provide hydrated calcium silicate crystal nucleus points for dicalcium silicate (C2S) and tricalcium silicate (C3S) silicate minerals in steel slag and steel slag sludge, and promote the earliest hydration of silicate minerals. The main components of mine tailings sludge, silicon dioxide (SiO2) and ferric oxide (Fe2O3), can play a role of dispersion, dilution, filling and skeleton in the cementitious system, which is conducive to the formation and accumulation of other cementitious products. The efficient synergistic hydration of multiple components promotes the super-superimposed hydration reaction of multi-component composite powder, making it have higher hydration activity and application effect.
[0039] At the same time, the active stimulant in this application only needs a small amount of addition to achieve a significant activation effect. First, the N,N-dimethylisopropanolamine in the active stimulant can complex the calcium ions in the silicate minerals in the active composite powder, and the N-dodecylethanolamine component can complex the calcium ions in the aluminate minerals in the active composite powder, promote the early hydration of silicate minerals and aluminate minerals and optimize the product; triisopropanolamine monoester sulfonate can promote the further development of the late strength of the active composite powder cementitious material; the glycerol polyoxypropylene ether component can eliminate the bubbles in the cementitious material and the bubbles caused by other admixture components, making the microstructure of the cementitious material more compact; the sodium thiosulfate component can promote the early strength of the cementitious material on the one hand, and on the other hand, it can also adjust the compatibility of the active composite powder with cement; the organic components in the active stimulant can also play a role in aiding grinding, dispersing and preventing agglomeration in the preparation process of the active composite powder of the present invention. The active stimulant of this application can generally effectively improve the promotion and application of active composite powder in different types of cement concrete.
[0040] The present application also provides a method for preparing an active composite powder based on steel slag or slag, the method comprising:
[0041] Step 1: pre-treating steel slag, ore slag, steel tailings mud, and mine tailings mud respectively to obtain steel slag powder, ore slag powder, steel tailings mud, and mine tailings mud;
[0042] The specific steps of pretreatment are as follows: steel slag, ore slag, steel tailings mud and mine tailings mud are crushed by fine crusher respectively; the crushed particles are subjected to magnetic separation to remove slag iron, and the powder after removing slag iron is pre-grinded to obtain steel slag powder, ore slag powder, steel tailings mud and mine tailings mud; after pre-grinding, the specific surface area of the steel slag powder is 430-600m 2 / kg, particle size is less than 60μm; the specific surface area of slag powder is 430~600m 2 / kg, particle size is less than 60μm; the specific surface area of steel tailings sludge is 450~550m 2 / kg, particle size less than 45μm; the specific surface area of mine tailings powder is 450~550m 2 / kg, particle size is less than 45μm.
[0043] Step 2: uniformly mixing 20 to 50 parts of steel slag powder, 40 to 70 parts of slag powder, 5 to 15 parts of steel tailings powder and 0 to 10 parts of mine tailings powder obtained after pretreatment to obtain a mixed solid powder;
[0044] Step 3: using a mixed solvent prepared from 2 to 15 parts of triisopropanolamine maleate sulfonate, 0 to 15 parts of N-dodecylethanolamine, 5 to 15 parts of N,N-dimethylisopropanolamine, 0 to 1 part of propylene glycol polyoxypropylene ether, 10 to 20 parts of sodium thiosulfate, and 40 to 70 parts of water as an active stimulant;
[0045] Step 4: Take 0-0.2 parts of active stimulant and spray or sprinkle evenly on the mixed solid powder, then transfer to the grinder and grind to a specific surface area of 450-550m 2 / kg, and the active composite powder is obtained.
[0046] The present invention is further described below with reference to the embodiments, but the present invention can be implemented in many different ways as defined and covered by the claims.
[0047] Example 1
[0048] The steel slag, mineral slag and steel tailings mud are respectively crushed by a fine crusher, magnetically separated and pre-grinded to obtain steel slag powder, mineral slag powder and steel tailings mud, so that the particle size of the steel slag powder and mineral slag powder is less than 60μm, the particle size of the steel tailings mud is less than 45μm, and the specific surface area reaches 470±10m 2 / kg(Steel slag powder), 440±10m 2 / kg(slag powder), 530±10m 2 / kg (steel tailings powder mud); steel slag powder, slag powder, and steel tailings powder mud are uniformly mixed in a ratio of 20 parts, 70 parts, and 10 parts to obtain a mixed solid powder; the mixed solid powder is ground in a mill to a specific surface area of 480±10m 2 / kg of micro powder to obtain active composite powder with an activity level of 95.
[0049] Example 2
[0050] The steel slag, mineral slag and steel tailings mud are respectively crushed by a fine crusher, magnetically separated and pre-grinded to obtain steel slag powder, mineral slag powder and steel tailings mud, so that the particle size of the steel slag powder and mineral slag powder is less than 60μm, the particle size of the steel tailings mud is less than 45μm, and the specific surface area reaches 470±10m 2 / kg(Steel slag powder), 440±10m 2 / kg(slag powder), 530±10m 2 / kg (steel tailings powder mud); steel slag powder, slag powder, and steel tailings powder mud are uniformly mixed in a ratio of 20 parts, 70 parts, and 10 parts to obtain a mixed solid powder;
[0051] Take 5 parts of triisopropanolamine maleate sulfonate, 12 parts of N-dodecylethanolamine, 8 parts of N,N-dimethylisopropanolamine, 0.2 parts of propylene glycol polyoxypropylene ether, 15 parts of sodium thiosulfate and 59.8 parts of water, and mix them evenly to prepare an active stimulant; spray 0.08 parts of the active stimulant evenly on the above mixed solid powder, and grind it in a mill to a specific surface area of 480±10m 2 / kg of micro powder to obtain active composite powder with an activity level of 95.
[0052] Example 3
[0053] Compared with Example 2, Example 3 is different in that 15 parts of triisopropanolamine maleate sulfonate, 5 parts of N-dodecylethanolamine, 5 parts of N,N-dimethylisopropanolamine, 0.2 parts of propylene glycol polyoxypropylene ether, 18 parts of sodium thiosulfate and 56.8 parts of water are evenly mixed to prepare an active stimulant, and the rest of the settings are the same as Example 3.
[0054] Example 4
[0055] The steel slag, ore slag, steel tailings mud and mine tailings mud are respectively crushed by a fine crusher, magnetic separation and pre-grinding to obtain steel slag powder, ore slag powder, steel tailings mud and mine tailings mud, so that the particle size of the steel slag powder and ore slag powder is less than 60μm, the particle size of the steel tailings mud and mine tailings mud is less than 45μm, and the specific surface area reaches 470±10m 2 / kg(Steel slag powder), 440±10m 2 / kg(slag powder), 530±10m 2 / kg(steel tailings sludge), 510±10m 2 / kg (mine tailings powder mud); steel slag powder, slag powder, steel tailings powder mud, and mine tailings powder mud are uniformly mixed in a ratio of 20 parts, 70 parts, 5 parts, and 5 parts to obtain a mixed solid powder;
[0056] Take 5 parts of triisopropanolamine maleate sulfonate, 12 parts of N-dodecylethanolamine, 8 parts of N,N-dimethylisopropanolamine, 0.2 parts of propylene glycol polyoxypropylene ether, 15 parts of sodium thiosulfate and 59.8 parts of water, and mix them evenly to prepare an active stimulant; spray 0.12 parts of the active stimulant evenly on the above mixed solid powder, and grind it in a mill to a specific surface area of 480±10m 2 / kg of micro powder to obtain active composite powder with an activity level of 95.
[0057] Example 5
[0058] The steel slag, ore slag, steel tailings mud and mine tailings mud are respectively crushed by a fine crusher, magnetic separation and pre-grinding to obtain steel slag powder, ore slag powder, steel tailings mud and mine tailings mud, so that the particle size of the steel slag powder and ore slag powder is less than 60μm, the particle size of the steel tailings mud and mine tailings mud is less than 45μm, and the specific surface area reaches 470±10m 2 / kg(Steel slag powder), 440±10m 2 / kg(slag powder), 530±10m 2 / kg(steel tailings sludge), 510±10m 2 / kg (mine tailings powder mud); steel slag powder, slag powder, steel tailings powder mud, and mine tailings powder mud are uniformly mixed in a ratio of 38 parts, 50 parts, 7 parts, and 5 parts to obtain a mixed solid powder; and the mixed solid powder is ground in a mill to a specific surface area of 480±10m 2 / kg of micro powder to obtain active composite powder with an activity level of 75.
[0059] Example 6
[0060] The steel slag, ore slag, steel tailings mud and mine tailings mud are respectively crushed by a fine crusher, magnetic separation and pre-grinding to obtain steel slag powder, ore slag powder, steel tailings mud and mine tailings mud, so that the particle size of the steel slag powder and ore slag powder is less than 60μm, the particle size of the steel tailings mud and mine tailings mud is less than 45μm, and the specific surface area reaches 470±10m 2 / kg(Steel slag powder), 440±10m 2 / kg(slag powder), 530±10m 2 / kg(steel tailings sludge), 510±10m 2 / kg (mine tailings powder mud); steel slag powder, slag powder, steel tailings powder mud, and mine tailings powder mud are uniformly mixed in a ratio of 38 parts, 50 parts, 7 parts, and 5 parts to obtain a mixed solid powder;
[0061] Take 5 parts of triisopropanolamine maleate sulfonate, 12 parts of N-dodecylethanolamine, 8 parts of N,N-dimethylisopropanolamine, 0.2 parts of propylene glycol polyoxypropylene ether, 15 parts of sodium thiosulfate and 59.8 parts of water, and mix them evenly to prepare an active stimulant; spray 0.08 parts of the active stimulant evenly on the above mixed solid powder, and grind it in a mill to a specific surface area of 480±10m 2 / kg of micro powder to obtain active composite powder with an activity level of 75.
[0062] Example 7
[0063] The steel slag, ore slag, steel tailings mud and mine tailings mud are respectively crushed by a fine crusher, magnetic separation and pre-grinding to obtain steel slag powder, ore slag powder, steel tailings mud and mine tailings mud, so that the particle size of the steel slag powder and ore slag powder is less than 60μm, the particle size of the steel tailings mud and mine tailings mud is less than 45μm, and the specific surface area reaches 470±10m 2 / kg(Steel slag powder), 440±10m 2 / kg(slag powder), 530±10m 2 / kg(steel tailings sludge), 510±10m 2 / kg (mine tailings powder mud); steel slag powder, slag powder, steel tailings powder mud, and mine tailings powder mud are uniformly mixed in a ratio of 38 parts, 50 parts, 7 parts, and 5 parts to obtain a mixed solid powder;
[0064] Take 15 parts of triisopropanolamine maleate sulfonate, 5 parts of N-dodecylethanolamine, 5 parts of N,N-dimethylisopropanolamine, 0.2 parts of propylene glycol polyoxypropylene ether, 18 parts of sodium thiosulfate and 59.8 parts of water, and mix them evenly to prepare an active stimulant; spray 0.08 parts of the active stimulant evenly on the above mixed solid powder, and grind it in a mill to a specific surface area of 480±10m 2 / kg of micro powder to obtain active composite powder with an activity level of 75.
[0065] Example 8
[0066] The steel slag, ore slag, steel tailings mud and mine tailings mud are respectively crushed by a fine crusher, magnetic separation and pre-grinding to obtain steel slag powder, ore slag powder, steel tailings mud and mine tailings mud, so that the particle size of the steel slag powder and ore slag powder is less than 60μm, the particle size of the steel tailings mud and mine tailings mud is less than 45μm, and the specific surface area reaches 470±10m 2 / kg(Steel slag powder), 440±10m 2 / kg(slag powder), 530±10m 2 / kg(steel tailings sludge), 510±10m 2 / kg (mine tailings powder mud); steel slag powder, slag powder, steel tailings powder mud, and mine tailings powder mud are uniformly mixed in a ratio of 38 parts, 45 parts, 10 parts, and 7 parts to obtain a mixed solid powder;
[0067] Take 5 parts of triisopropanolamine maleate sulfonate, 12 parts of N-dodecylethanolamine, 8 parts of N,N-dimethylisopropanolamine, 0.2 parts of propylene glycol polyoxypropylene ether, 15 parts of sodium thiosulfate and 59.8 parts of water, and mix them evenly to prepare an active stimulant; spray 0.15 parts of the active stimulant evenly on the above mixed solid powder, and grind it in a mill to a specific surface area of 480±10m 2 / kg of micro powder to obtain active composite powder with an activity level of 75.
[0068] Comparative Example 1
[0069] The steel slag is crushed by a fine crusher, magnetically separated and pre-grinded to obtain steel slag powder, so that the particle size of the steel slag powder is less than 60μm and the specific surface area reaches 480±10m 2 / kg, as a single-component active micropowder.
[0070] Comparative Example 2
[0071] The steel slag and slag are crushed by a fine crusher, subjected to magnetic separation and pre-grinding to obtain steel slag powder and slag powder, and the particle size of the steel slag powder and slag powder is less than 60 μm; the steel slag powder and slag powder are uniformly mixed in 30 parts by mass and 70 parts by mass to obtain a mixed solid powder; the mixed solid powder is ground in a mill into a specific surface area of 480±10m 2 / kg of micronized powder was used as a comparison group for the active composite powder with an activity level of 95.
[0072] Comparative Example 3
[0073] The steel slag and slag are crushed by a fine crusher, subjected to magnetic separation and pre-grinding to obtain steel slag powder and slag powder, and the particle size of the steel slag powder and slag powder is less than 60 μm; the steel slag powder and slag powder are uniformly mixed in 50 parts by mass and 50 parts by mass to obtain a mixed solid powder; the mixed solid powder is ground in a mill into a specific surface area of 480±10m 2 / kg of micronized powder was used as a comparison group for the active composite powder with an activity level of 75.
[0074] The above Examples 1 to 8 and Comparative Examples 1 to 3 were subjected to activity index tests according to GB / T 28293-2012. The activity index obtained in the test was graded according to the activity index in the national standard GB / T 28293-2012. The experimental results are shown in Table 1.
[0075] Table 1
[0076]
[0077]
[0078] It can be seen from Table 1 above that the 7d and 28d activity indexes of the active composite powders of Examples 1 to 8 in the present application are significantly higher than those of Comparative Example 1 using a single component; at the same time, compared with Example 1 without adding an active stimulant, Examples 2 to 4 have higher 7d activity indexes and 28d activity indexes, with Examples 2 to 4 reaching level 95, while Example 1 is close to level 95, indicating that the addition of active additives can effectively improve the activity index and level of the active composite powder. Examples 5-8 all reached an activity index of level 75 or even level 85. Moreover, the activity indexes of the active composite powders of the examples with added active stimulants are also higher than those of the examples without added active stimulants, indicating that the active stimulants have a good promoting effect on the activity enhancement of the active composite powders.
[0079] Furthermore, application tests were conducted on some embodiments in concrete materials.
[0080] C30 grade concrete test was carried out according to the concrete mix proportion shown in Table 2.
[0081] Table 2
[0082]
[0083] The comparison of concrete performance test results is shown in Table 3.
[0084] Table 3
[0085]
[0086] It can be seen from Table 3 that under the same conditions, the slump and early and late strength of the C30 concrete prepared by using the active composite powder in Example 3 of the present application are higher than those of the conventional C30 concrete, and the C30 concrete prepared by using the active composite powder in Example 3 of the present invention can reduce the amount of cement, and the cement amount reduction rate is 8.3%, which not only reduces the cost, but also is conducive to the reduction of carbon emissions of concrete. It shows that the active composite powder of the present application is used as an admixture in concrete and shows good use effect, and can be used as a concrete admixture in the production and preparation of cement concrete.
[0087] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present invention without departing from the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. An active composite powder based on steel slag or slag, characterized in that: The active composite powder comprises the following components in parts by mass: 20-50 parts of steel slag powder, 40-70 parts of slag powder, 5-15 parts of steel tailings powder mud, 0-10 parts of mine tailings powder mud and 0-0.2 parts of active activator; the components of the steel slag powder include dicalcium silicate, tricalcium silicate, tricalcium aluminate, calcium heptaaluminate, calcium oxide and magnesium oxide minerals; the slag powder contains active alumina and / or silicon dioxide amorphous glass minerals; the steel tailings powder mud contains calcium oxide, silicon dioxide, ferric oxide, tricalcium silicate, dicalcium silicate, calcium ferrite and hydrated calcium silicate; the mine tailings powder mud contains silicon dioxide and ferric oxide; Among them, the active stimulant is composed of 2 to 15 parts of triisopropanolamine maleate sulfonate, 5 to 15 parts of N-dodecylethanolamine, 5 to 15 parts of N,N-dimethylisopropanolamine, 0.2 to 1 part of propylene glycol polyoxypropylene ether, 10 to 20 parts of sodium thiosulfate and 40 to 70 parts of water, calculated by mass.
2. The active composite powder based on steel slag or slag according to claim 1, characterized in that: The specific surface area of the steel slag powder is 430~600m 2 / kg, particle size is less than 60μm.
3. The active composite powder based on steel slag or slag according to claim 1, characterized in that: The specific surface area of the slag powder is 430~600m 2 / kg, particle size is less than 60μm.
4. The active composite powder based on steel slag or slag according to claim 1, characterized in that: The specific surface area of steel tailings sludge is 450~550m 2 / kg, particle size is less than 45μm.
5. The active composite powder based on steel slag or slag according to claim 1, characterized in that: The specific surface area of the mine tailings powder is 450~550m 2 / kg, particle size is less than 45μm.
6. The active composite powder based on steel slag or slag according to claim 1, characterized in that: The specific surface area of the active composite powder is 450-550 m 2 / kg.
7. The active composite powder based on steel slag or slag according to any one of claims 1 to 6, characterized in that: The 7d activity index of the active composite powder is not less than 60%.
8. The active composite powder based on steel slag or slag according to claim 7, characterized in that: The 28d activity index of the active composite powder is not less than 75%.
9. A method for preparing an active composite powder based on steel slag or slag according to any one of claims 1 to 8, characterized in that: The preparation method comprises: Step 1: pre-treating steel slag, ore slag, steel tailings mud and mine tailings mud respectively to obtain steel slag powder, ore slag powder, steel tailings mud and mine tailings mud; the components of the steel slag powder include dicalcium silicate, tricalcium silicate, tricalcium aluminate, calcium heptaaluminate, calcium oxide and magnesium oxide minerals; the slag powder contains active alumina and / or silicon dioxide amorphous glass minerals; the steel tailings mud contains calcium oxide, silicon dioxide, ferric oxide, tricalcium silicate, dicalcium silicate, calcium ferrite and hydrated calcium silicate; the mine tailings mud contains silicon dioxide and ferric oxide; Step 2: By weight, 20-50 parts of steel slag powder, 40-70 parts of slag powder, 5-15 parts of steel tailings powder and 0-10 parts of mine tailings powder obtained after pretreatment are uniformly mixed to obtain a mixed solid powder; Step 3: Using 2 to 15 parts of triisopropanolamine maleate sulfonate, 5 to 15 parts of N-dodecylethanolamine, 5 to 15 parts of N,N-dimethylisopropanolamine, 0.2 to 1 parts of propylene glycol polyoxypropylene ether, 10 to 20 parts of sodium thiosulfate, and 40 to 70 parts of water as a mixed solvent as an active stimulant, by weight; Step 4: Take 0~0.2 parts of active stimulant and spray or sprinkle evenly on the mixed solid powder, then transfer to the grinder and grind to a specific surface area of 450~550m 2 / kg, and the active composite powder is obtained.
10. The method for preparing active composite powder based on steel slag or slag according to claim 9, characterized in that: The specific preprocessing of step one is: The steel slag, ore slag, steel tailings mud and mine tailings mud are crushed by fine crushers respectively; the crushed particles are subjected to magnetic separation to remove the slag iron therein, and the powder after the slag iron is removed is pre-grinded to obtain steel slag powder, ore slag powder, steel tailings mud and mine tailings mud; wherein the steel slag powder is pre-grinded to a specific surface area of 430-600m 2 / kg, with a particle size of less than 60μm; the slag powder is pre-ground to a specific surface area of 430~600m 2 / kg, particle size less than 60μm; steel tailings powder is pre-ground to a specific surface area of 450~550m 2 / kg, particle size is less than 45μm; the mine tailings powder is pre-ground to a specific surface area of 450~550m 2 / kg, particle size is less than 45μm.
Citation Information
Patent Citations
Compound active powder of ball milling steel slag tailing slurry and blast-furnace slag and application of compound active powder in preparing concrete
CN101544479A
High-activity iron and steel slag powder and preparation method thereof
CN105399349A
Tailing-based cementing material and preparation method thereof
CN111847924A