A Pt-based single-atom catalyst for dehydrogenating propane to produce propylene and a preparation method thereof
By impregnating Pt, Sn and Ba on the alumina support, the PtSnBa/Al2O3 catalyst is formed, which solves the problem of sintering and inactivation of Pt-based catalysts at high temperatures, and achieves high stability and renewability of the catalyst, avoiding the chlorine regeneration belt The risk of coming reduces the cost.
Patent Information
- Application Number
- CN202310348971.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-04-04
AI Technical Summary
The existing Pt-based catalysts are prone to sintering and inactivated under high temperature conditions, and require frequent chlorine regeneration treatment, which poses environmental and safety risks and is costly.
Alumina is used as a support and Pt, Sn and Ba are introduced by impregnation method to form PtSnBa/Al2O3 catalyst. Pt exists in a single atom form and has ultra-high thermal stability. Carbon deposition occurs only at high temperatures, and the catalyst after the fire passes through It can be regenerated by burning air.
The long-term stability and high activity of the catalyst are achieved, the environmental and safety risks brought about by chlorine regeneration are avoided, the costs are reduced, and the anti-sintering performance and regeneration ability of the catalyst are improved.
Smart Images

Figure CN116510727B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of propane dehydrogenation to propylene catalyst, and particularly relates to a Pt-based single-atom catalyst for propane dehydrogenation to propylene and a preparation method thereof. Background Art
[0002] Propylene is an important organic compound, which is a colorless, odorless, slightly sweet gas at room temperature. Propylene has a rich downstream industrial chain. It can be used to produce acrylonitrile, propylene oxide, isopropanol, phenol, acetone, butanol, octanol, acrylic acid and its esters, propylene glycol, epichlorohydrin and synthetic glycerol. Propylene is also one of the most basic raw materials for plastics, synthetic rubber and synthetic fibers.
[0003] At present, the main sources of propylene are oil route, natural gas route and coal route. The oil route includes catalytic cracking (FCC) and steam cracking, which is the main production process of propylene in my country, accounting for about 55% of the market, but it has disadvantages such as complex separation process, large investment, and low propylene yield; relying on my country's abundant coal resources, although coal-to-olefins has developed rapidly, it has disadvantages such as complex reaction process, large consumption of water, and high energy consumption. The natural gas route, namely propane dehydrogenation, can obtain significantly higher propylene yield and high propylene selectivity under high temperature and low pressure conditions, and with the successful exploitation of shale gas, it has a cheap and sufficient source of raw materials. Therefore, propane dehydrogenation technology has obvious advantages in terms of cost, energy consumption, environmental protection, propylene yield and selectivity, and has been a research hotspot in recent years.
[0004] After more than 20 years of development, propane dehydrogenation technology currently has eight major processes worldwide, and the catalysts used are also different. Among them, Cr-based catalysts represented by the Catofin process and Pt-based catalysts represented by the Oleflex process are the most widely used. Cr-based catalysts are inexpensive, but the Cr element has a large impact on the environment, and its prospects for use are greatly limited; Pt-based catalysts have high catalytic activity and excellent propylene selectivity, and are environmentally friendly, and have gradually become the mainstream catalyst for PDH. Limited by thermodynamic equilibrium, the propane dehydrogenation reaction needs to be carried out at high temperatures to achieve a high single-pass propane conversion rate. However, high temperature conditions will promote the occurrence of adverse side reactions such as deep dehydrogenation and cracking of propane, resulting in rapid sintering and coking of the catalyst and deactivation. Therefore, the Pt-based catalyst needs to be regenerated every 7 to 10 days.
[0005] The economic cost of the precious metal Pt has prompted the development of a regeneration method for the sintering problem of supported catalysts. The oxychlorination reaction based on halogens (mainly chlorine) is the most effective regeneration method, which redisperses the sintered metal particles on the carrier, thereby reducing the metal particle size and restoring the catalytic activity. A similar method is also used to regenerate the catalyst in the Oleflex process. The entire process includes charring the Pt-based catalyst under different oxygen concentrations and redispersing the Pt with chlorine. This process can not only remove carbon deposits, but also redisperse the agglomerated Pt particles, ultimately restoring the activity of the catalyst. Since chlorine is a highly toxic chemical that is harmful to the environment and the human body, and its reaction activity is extremely strong and highly corrosive to reaction equipment; therefore, the transportation, storage, use and exhaust gas treatment of chlorine are not only costly, but also have certain risks and great insecurity in its management and operation. Therefore, the industry is in urgent need of developing new anti-sintering catalysts that can achieve catalyst regeneration without the use of chlorine. To this end, the present invention has developed a propane dehydrogenation Pt-based single-atom catalyst, in which Pt exists on the surface of an alumina carrier in the form of a single atom under the promotion of the additive Ba. The single-atom Pt has ultra-high thermal stability and does not sinter under high-temperature reaction conditions. The catalyst is only deactivated by carbon deposition, and the catalyst after the fire can be regenerated by simple air roasting. Summary of the invention
[0006] The purpose of the present invention is to provide a Pt-based single-atom catalyst for propane dehydrogenation to propylene in view of the poor stability of Pt catalysts and the sintering deactivation. The catalyst is a supported catalyst, using alumina as a carrier, and introducing active components Pt and a first auxiliary agent Sn and a second auxiliary agent Ba by an impregnation method. Compared with other catalysts, the prepared catalyst has extremely strong anti-sintering ability, only sintering deactivation occurs during the reaction, and the catalyst after the fire can be regenerated by simple air roasting, so the catalyst has good industrial application prospects.
[0007] To achieve the above object, the technical solution of the present invention is:
[0008] A Pt-based single-atom catalyst for dehydrogenating propane to propylene, expressed as PtSnBa / Al2O3, wherein the active component is Pt, Sn is a first auxiliary agent, Ba is a second auxiliary agent, and Al2O3 is used as a carrier; wherein the mass percentage of the active component Pt is 0.2-0.4%, the mass percentage of the first auxiliary agent Sn is 0.1-0.3%, the weight percentage of the second auxiliary agent Ba is 1.0-3.0%, and the rest is Al2O3.
[0009] The preparation method of the above-mentioned Pt-based single-atom catalyst for dehydrogenation of propane to propylene is to adopt an impregnation method, and the steps are as follows:
[0010] (1) dissolving a Pt source, a Sn source and a Ba source in an alcohol solvent and / or a water solvent to obtain an impregnation solution;
[0011] (2) The impregnation solution is impregnated onto an Al2O3 carrier, and then dried, calcined, and reduced to obtain a Pt-based single-atom catalyst for dehydrogenation of propane to produce propylene.
[0012] Furthermore, the Sn source in step (1) is tin dichloride, and the Ba source is one of barium nitrate, barium chloride, barium hydroxide, barium sulfate, barium bromide, barium acetate, and barium titanate. The mass ratio of the impregnation solution to the Al2O3 carrier is 1:1-4:1; the impregnation time is 1-20h. It is characterized in that: the drying temperature in step (2) is 50-150°C, and the drying time is 3-12h. The calcination temperature in step (2) is 200-550°C, and the calcination time in step (2) is 3-12h; the reduction temperature is 400°C to 600°C; the gases used in the reduction reaction are nitrogen and hydrogen, wherein the volume flow ratio of nitrogen to hydrogen is 1:(0~0.3) and is not 0.
[0013] Application of the above-mentioned Pt-based single-atom catalyst for propane dehydrogenation to propylene: The propane dehydrogenation to propylene reaction is carried out in a fixed bed reactor at a reaction temperature of 590°C, and the reaction gas is introduced into the reactor loaded with the Pt-based single-atom catalyst for propane dehydrogenation to propylene.
[0014] Beneficial effects of the present invention: The catalyst provided by the present invention not only has high activity, but also has extremely strong anti-sintering performance. The conversion rate and selectivity of the deactivated catalyst can be completely restored by simple air roasting. For the catalyst without Ba additive, the selectivity and conversion rate of the PtSn / Al2O3 catalyst continue to decline after five regenerations; after the introduction of Ba additive, the conversion rate and selectivity of the PtSnBa / Al2O3 catalyst can be completely restored or even higher after eight regenerations; this technology has significant results in improving the stability of the catalyst.
[0015] Description of the accompanying tables and graphs
[0016] Figure 1 This is a high-resolution transmission electron microscopy (TEM) image of PtSnBa / Al2O3 prepared in Example 2 before reaction;
[0017] Figure 2 This is a high-resolution transmission electron microscopy (TEM) image of PtSnBa / Al2O3 prepared in Example 2 after 8 consecutive reactions and regenerations. DETAILED DESCRIPTION
[0018] The technical solution of the present invention is described in detail below in conjunction with embodiments, but the present invention is not limited to the following embodiments.
[0019] Example 1 (without Ba added as comparison)
[0020] Weigh 2.5g of alumina balls, weigh an appropriate amount of tin dichloride to prepare an ethanol solution, then add the above carrier to the tin dichloride solution, soak at 40℃ for 10h, dry at 80℃ for 5h, and calcine at 350℃ for 2h; weigh an appropriate amount of chloroplatinic acid (calculate the amount of chloroplatinic acid based on the Pt loading of 0.30%) to prepare an aqueous solution, place the calcined carrier in the chloroplatinic acid aqueous solution and add an appropriate amount of hydrochloric acid, soak at 40℃ for 10h, then dry at 80℃ for 5h, and calcine at 300℃ for 4h; the obtained catalyst precursor is reduced at 570℃ and 20 vol% hydrogen atmosphere for 1h to obtain Pt-Sn / Al2O3 catalyst. 1g of the obtained catalyst is loaded in a fixed bed tubular reactor, and propane is used as the reactant. The reaction is carried out at 590℃, normal pressure, and a hydrogen-to-hydrocarbon ratio of 1 / 2. Carbonization regeneration is carried out at 480℃, 2% oxygen atmosphere and 520℃, 10% oxygen atmosphere.
[0021] Example 2
[0022] Weigh 2.5 g of alumina balls, weigh an appropriate amount of tin dichloride to prepare an ethanol solution, then add the above-mentioned carrier to the tin dichloride solution, soak at 40°C for 10 hours, dry at 80°C for 5 hours, and calcine at 350°C for 2 hours; weigh an appropriate amount of chloroplatinic acid (the amount of chloroplatinic acid is calculated based on the Pt loading of 0.30%) and barium nitrate to prepare an aqueous solution, place the calcined carrier in a barium nitrate-chloroplatinic acid aqueous solution (Ba / Pt=1) and add an appropriate amount of hydrochloric acid, soak at 40°C for 10 hours, then dry at 80°C for 5 hours, and calcine at 300°C for 4 hours; the obtained catalyst precursor is reduced at 570°C and 20 vol% hydrogen atmosphere for 1 hour to obtain a Pt-Sn-Ba / Al2O3 catalyst. 1 g of the obtained catalyst was loaded into a fixed bed tubular reactor, and propane was used as the reactant. The reaction was carried out at 590°C, normal pressure, and a hydrogen-to-hydrocarbon ratio of 1 / 2. Carbonization regeneration was carried out at 480°C, 2% oxygen atmosphere, and 520°C, 10% oxygen atmosphere.
[0023] Example 3
[0024] Weigh 2.5 g of alumina balls, weigh an appropriate amount of tin dichloride to prepare an ethanol solution, then add the above-mentioned carrier to the tin dichloride solution, soak at 40°C for 10 hours, dry at 80°C for 5 hours, and calcine at 350°C for 2 hours; weigh an appropriate amount of chloroplatinic acid (the amount of chloroplatinic acid is calculated based on the Pt loading of 0.25%) and barium acetate to prepare an aqueous solution, place the calcined carrier in a barium acetate-chloroplatinic acid aqueous solution (Ba / Pt=2) and add an appropriate amount of hydrochloric acid, soak at 40°C for 10 hours, then dry at 80°C for 5 hours, and calcine at 300°C for 4 hours; the obtained catalyst precursor is reduced at 570°C and 20 vol% hydrogen atmosphere for 1 hour to obtain a Pt-Sn-Ba / Al2O3 catalyst. 1 g of the obtained catalyst was loaded into a fixed bed tubular reactor, and propane was used as the reactant. The reaction was carried out at 590°C, normal pressure, and a hydrogen-to-hydrocarbon ratio of 1 / 2. Carbonization regeneration was carried out at 480°C, 2% oxygen atmosphere, and 520°C, 10% oxygen atmosphere.
[0025] Example 4
[0026] Weigh 2.5 g of alumina balls, weigh an appropriate amount of tin dichloride to prepare an ethanol solution, then add the above-mentioned carrier to the tin dichloride solution, soak at 40°C for 10 hours, dry at 80°C for 5 hours, and calcine at 350°C for 2 hours; weigh an appropriate amount of chloroplatinic acid (the amount of chloroplatinic acid is calculated based on the Pt loading of 0.28%) and barium hydroxide to prepare an aqueous solution, place the calcined carrier in a barium hydroxide-chloroplatinic acid aqueous solution (Ba / Pt=3) and add an appropriate amount of hydrochloric acid, soak at 40°C for 10 hours, then dry at 80°C for 5 hours, and calcine at 300°C for 4 hours; the obtained catalyst precursor is reduced at 570°C and 20 vol% hydrogen atmosphere for 1 hour to obtain a Pt-Sn-Ba / Al2O3 catalyst. 1 g of the obtained catalyst was loaded into a fixed bed tubular reactor, and propane was used as the reactant. The reaction was carried out at 590°C, normal pressure, and a hydrogen-to-hydrocarbon ratio of 1 / 2. Carbonization regeneration was carried out at 480°C, 2% oxygen atmosphere, and 520°C, 10% oxygen atmosphere.
[0027] Example 5
[0028] Weigh 2.5 g of alumina beads, weigh an appropriate amount of tin dichloride to prepare an ethanol solution, then add the above-mentioned carrier to the tin dichloride solution, soak at 40°C for 10 hours, dry at 80°C for 5 hours, and calcine at 350°C for 2 hours; weigh an appropriate amount of chloroplatinic acid (the amount of chloroplatinic acid is calculated based on the Pt loading of 0.35%) and strontium nitrate to prepare an aqueous solution, place the calcined carrier in a barium sulfate-chloroplatinic acid aqueous solution (Ba / Pt=4) and add an appropriate amount of hydrochloric acid, soak at 40°C for 10 hours, then dry at 80°C for 5 hours, and calcine at 300°C for 4 hours; the obtained catalyst precursor is reduced at 570°C and 20 vol% hydrogen atmosphere for 1 hour to obtain a Pt-Sn-Ba / Al2O3 catalyst. 1 g of the obtained catalyst was loaded into a fixed bed tubular reactor, and propane was used as the reactant. The reaction was carried out at 590°C, normal pressure, and a hydrogen-to-hydrocarbon ratio of 1 / 2. Carbonization regeneration was carried out at 480°C, 2% oxygen atmosphere, and 520°C, 10% oxygen atmosphere.
[0029] Example 6
[0030] Weigh 2.5 g of alumina balls, weigh an appropriate amount of tin dichloride to prepare an ethanol solution, then add the above-mentioned carrier to the tin dichloride solution, soak at 40°C for 10 hours, dry at 80°C for 5 hours, and calcine at 350°C for 2 hours; weigh an appropriate amount of chloroplatinic acid (the amount of chloroplatinic acid is calculated based on the Pt loading of 0.40%) and barium nitrate to prepare an aqueous solution, place the calcined carrier in a barium bromide-chloroplatinic acid aqueous solution (Ba / Pt=5) and add an appropriate amount of citric acid, soak at 40°C for 10 hours, then dry at 80°C for 5 hours, and calcine at 300°C for 4 hours; the obtained catalyst precursor is reduced at 570°C and 20 vol% hydrogen atmosphere for 1 hour to obtain a Pt-Sn-Ba / Al2O3 catalyst. 1 g of the obtained catalyst was loaded into a fixed bed tubular reactor, and propane was used as the reactant. The reaction was carried out at 590°C, normal pressure, and a hydrogen-to-hydrocarbon ratio of 1 / 2. Carbonization regeneration was carried out at 480°C, 2% oxygen atmosphere, and 520°C, 10% oxygen atmosphere.
[0031] Example 7
[0032] Weigh 2.5 g of alumina balls, weigh an appropriate amount of tin dichloride to prepare an ethanol solution, then add the above-mentioned carrier to the tin dichloride solution, soak at 40°C for 10 hours, dry at 80°C for 5 hours, and calcine at 350°C for 2 hours; weigh an appropriate amount of chloroplatinic acid (the amount of chloroplatinic acid is calculated based on the Pt loading of 0.20%) and barium nitrate to prepare an aqueous solution, place the calcined carrier in a barium titanate-chloroplatinic acid aqueous solution (Ba / Pt=6) and add an appropriate amount of acetic acid, soak at 40°C for 10 hours, then dry at 80°C for 5 hours, and calcine at 300°C for 4 hours; the obtained catalyst precursor is reduced at 570°C and 20 vol% hydrogen atmosphere for 1 hour to obtain a Pt-Sn-Ba / Al2O3 catalyst. 1 g of the obtained catalyst was loaded into a fixed bed tubular reactor, and propane was used as the reactant. The reaction was carried out at 590°C, normal pressure, and a hydrogen-to-hydrocarbon ratio of 1 / 2. Carbonization regeneration was carried out at 480°C, 2% oxygen atmosphere, and 520°C, 10% oxygen atmosphere.
[0033] Figure 1 This is a high-resolution transmission electron microscopy (TEM) image of PtSnBa / Al2O3 before the reaction. From the image, it can be seen that Pt is highly dispersed on the surface of the carrier and exists on the surface of Al2O3 in the form of single atoms. Figure 2 High-resolution transmission electron microscopy (TEM) image of PtSnBa / Al2O3 after 8 consecutive reactions and regenerations. Figure 2 It can be seen that the Pt single atoms on the Al2O3 surface have ultra-high stability. After PtSnBa / Al2O3 was reacted 9 times at 590℃ and regenerated 8 times at 520℃, the Pt single atoms did not agglomerate. Figure 1 and Figure 2 By comparison, it can be seen that the PtSnBa / Al2O3 catalyst prepared by the patent of the present invention has a strong anti-sintering ability. After multiple reactions and regenerations, no agglomeration of Pt single atoms occurs.
[0034] From the comparison in Table 1, it can be seen that the PtSnBa / Al2O3 catalyst prepared by the present invention shows excellent anti-sintering performance, and no irreversible sintering deactivation occurs during the reaction. In Example 1, no Ba additive is added. From the data, it can be seen that the activity of the catalyst gradually decreases with the increase in the number of regenerations, indicating that the catalyst is non-regenerative. In Examples 2-7, Ba additives are introduced. From the data, it can be seen that the catalyst has excellent regeneration performance, and the deactivated catalyst can be completely regenerated after simple oxygen treatment.
[0035] Table 1 Propane conversion data of the catalyst prepared in Example after 8 consecutive reactions and regeneration
[0036]
[0037] The above embodiments describe the present invention in detail, but they are only examples and do not limit the patent scope of the present invention. Any equivalent modification and substitution of the present invention using the present description is also within the scope of the present invention and is included in the patent protection scope of the present invention.
Claims
1. A Pt-based single-atom catalyst for dehydrogenation of propane to propylene, characterized in that: The catalyst is expressed as PtSnBa / Al2O3, wherein the active component is Pt, Sn is the first auxiliary agent, Ba is the second auxiliary agent, and Al2O3 is used as a carrier; wherein the mass percentage of the active component Pt is 0.2-0.4%, the mass percentage of the first auxiliary agent Sn is 0.1-0.3%, the weight percentage of the second auxiliary agent Ba is 1.0-3.0%, and the rest is Al2O3; The catalyst is prepared by an impregnation method, and the steps are as follows: (1) dissolving a Pt source, a Sn source and a Ba source in an alcohol solvent and / or a water solvent to obtain an impregnation solution; the Sn source is tin dichloride, and the Ba source is one of barium nitrate, barium chloride, barium hydroxide, barium sulfate, barium bromide, barium acetate and barium titanate; (2) The impregnation solution is impregnated onto an Al2O3 carrier, and then dried, calcined, and reduced to obtain a Pt-based single-atom catalyst for dehydrogenation of propane to produce propylene.
2. The Pt-based single-atom catalyst for dehydrogenating propane to propylene according to claim 1, characterized in that: The mass ratio of the impregnation solution to the Al2O3 carrier is 1:1-4:1, and the impregnation time is 1-20 h.
3. The Pt-based single-atom catalyst for dehydrogenating propane to propylene according to claim 1, characterized in that: The drying temperature in step (2) is 50-150° C. and the drying time is 3-12 h.
4. The Pt-based single-atom catalyst for dehydrogenation of propane to propylene according to claim 1, characterized in that: The calcination temperature in step (2) is 200-550° C., and the calcination time in step (2) is 3-12 h.
5. The Pt-based single-atom catalyst for dehydrogenation of propane to propylene according to claim 1, characterized in that: The reduction temperature in step (2) is 400°C to 600°C.
6. The Pt-based single-atom catalyst for dehydrogenation of propane to propylene according to claim 1, characterized in that: The gases used in the reduction reaction in step (2) are nitrogen and hydrogen, wherein the volume flow ratio of nitrogen to hydrogen is 1:(0-0.3) and is not 0.
7. An application of the Pt-based single-atom catalyst for dehydrogenation of propane to propylene as claimed in claim 1, characterized in that: The propane dehydrogenation to propylene reaction is carried out in a fixed bed reactor at a reaction temperature of 590° C. The reaction gas is introduced into a reactor loaded with a Pt-based single-atom catalyst for propane dehydrogenation to propylene.
Citation Information
Patent Citations
Anti-carbon deposition platinum-based catalyst for preparing propylene through propane dehydrogenation and preparation method thereof
CN106512994A
Platinum-based catalyst for preparing propylene through propane dehydrogenation and preparation method of platinum-based catalyst
CN110237849A
Pt-based multi-component catalyst for preparing propylene by propane dehydrogenation, and preparation method thereof
CN111790384A
Catalyst for preparing propylene by propane dehydrogenation, preparation method therefor, and use thereof
WO2021128867A1