A kind of efflorescence inhibitor and its preparation process and application in silica-alumina gelling material

Nanomodified ammonium stearate emulsion inhibits the phenomenon of alkaline in silicon-aluminum gelling materials, solving the problems of degradation of the mechanical properties of the materials and application limitations, and achieving a significant improvement in the anti-alkali and durability.

CN116514434BActive Publication Date: 2024-11-22UNIV OF JINAN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310500640.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-06
Publication Date
2024-11-22
Estimated Expiration
2043-05-06

AI Technical Summary

Technical Problem

Silicon-aluminum gelling materials are prone to alkaline-polying, resulting in degradation of the mechanical properties of the materials and limited application. The existing densification or hydrophobic treatment cannot be effectively suppressed for a long time.

Method used

Using nano-modified ammonium stearate emulsion, two nano-modified stearic acids were prepared by loading ammonium stearate on mesoporous nanomaterials and combining them with van der Waals force to form an emulsion. Combining surfactant emulsifiers and nanomaterials, two nano-modified stearic acids were prepared. Ammonium emulsion, used in silicon-aluminum gelling materials, significantly improving anti-alkali and durability.

Benefits of technology

While ensuring the mechanical properties of the material, the anti-alkali ability and durability of silicon-aluminum gelling materials are significantly improved, the difficulty of water-salt transmission is extended, the diffusion rate of alkali metal cations is reduced, the leachation is prevented, and the density of pore structure is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116514434B_ABST
    Figure CN116514434B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of alkali inhibitors, and specifically discloses an alkali-effluxing inhibitor, a preparation process thereof, and an application thereof in a silica-alumina gelling material. The alkali-effluxing inhibitor comprises two nano-modified ammonium stearate emulsions; wherein: the first nano-modified ammonium stearate emulsion is an emulsion in which ammonium stearate is loaded on a mesoporous nano-material and is formed by combining through van der Waals forces; the second nano-modified ammonium stearate emulsion is an emulsion system formed by ammonium stearate with a surface coated with a nano-particle material dispersed in an emulsion. The above-mentioned alkali-effluxing inhibitor of the present invention utilizes a technical solution in which ammonium stearate is loaded on a mesoporous nano-material and is formed by combining through van der Waals forces to solidify alkali metal cations in a silica-alumina gelling material, thereby being able to significantly improve the alkali-effluxing resistance and durability of the silica-alumina substrate while ensuring that the material has excellent mechanical properties, thereby greatly improving the quality of the building and the aesthetic and durability of the appearance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alkali inhibitors, and in particular to an alkali-efflux inhibitor and a preparation process thereof and application thereof in silica-alumina gelling materials. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Silica-alumina cementitious materials are hydraulic cementitious materials made by physical and chemical stimulation, with slag, fly ash, phosphorus slag and other industrial waste residues or natural minerals such as volcanic ash and zeolite as the main raw materials. Compared with the traditional cement production process, the preparation process of silica-alumina cementitious materials is simple, does not require calcination and consumption of mineral resources such as limestone, which can greatly reduce production energy consumption and reduce carbon dioxide emissions; at the same time, it can make full use of industrial wastes such as steel slag, fly ash, slag, and coal gangue, providing an effective way for the resource utilization of these wastes. The emergence of silica-alumina cementitious materials just meets the development needs of modern society for new materials, and it is considered to be a new type of structural material with good development prospects. However, the internal soluble alkali content of silica-alumina cementitious materials is too high, the internal metal ion activity is high, and the weak binding of active alkali metal ions in the gel structure makes it easy to leach from the pore structure, and may have a certain corrosive effect on the slag and the metal frame in the concrete. One of the main factors limiting the application of silica-alumina cementitious materials is alkali dissolution, that is, alkali efflorescence.

[0004] At present, commonly used methods to inhibit efflorescence include hydrophobic modification of the sample surface, optimization of pore size distribution, etc. However, on the one hand, simple densification or waterproofing treatment methods have little effect and cannot maintain the long-term efflorescence inhibition effect. For the densification treatment or surface hydrophobic treatment of silica-alumina cementitious materials, their efflorescence inhibition effect often faces the problem of irreversible decline with the increase of service time, and the efflorescence phenomenon cannot be fundamentally solved. On the other hand, the overall hydrophobic treatment makes it difficult to maintain the mechanical properties of silica-alumina cementitious materials. This method achieves the function of inhibiting water and salt transmission by adding hydrophobic agents, but the addition of hydrophobic agents often causes a significant deterioration of the mechanical properties of the material, which brings considerable limitations to the application of this material. Summary of the invention

[0005] The present invention provides an efflorescence inhibitor and a preparation process thereof and an application thereof in a silicon-aluminum gelling material. The efflorescence inhibitor can significantly improve the efflorescence resistance and durability of the silicon-aluminum substrate while ensuring that the material has excellent mechanical properties, thereby improving the quality, aesthetic appearance and durability of the building. To achieve the above purpose, the present invention provides the following technical solution.

[0006] In a first aspect, the present invention discloses an alkali-releasing inhibitor, comprising two nano-modified ammonium stearate emulsions. The first nano-modified ammonium stearate emulsion is an emulsion in which ammonium stearate is loaded on a mesoporous nanomaterial and combined by van der Waals forces. The second nano-modified ammonium stearate emulsion is an emulsion system in which ammonium stearate with a surface coated with nanoparticle material is dispersed in an emulsion. The mass ratio of the first nano-modified ammonium stearate emulsion to the second nano-modified ammonium stearate emulsion is 1:1 to 3.

[0007] Furthermore, the raw material composition of the first nano-modified ammonium stearate emulsion includes: 20-30 parts by weight of stearic acid, 2-3 parts by weight of surfactant emulsifier, 20-25 parts by weight of ammonia water, 0.1-0.25 parts by weight of mesoporous nanomaterial, and 35-45 parts by weight of water.

[0008] Furthermore, the raw material composition of the second nano-modified ammonium stearate emulsion includes: 20-30 parts by weight of stearic acid, 2-3 parts by weight of surfactant emulsifier, 20-25 parts by weight of ammonia water, 0.1-0.25 parts by weight of nanomaterial, and 35-45 parts by weight of water.

[0009] Further, the surface active emulsifier includes but is not limited to: one or more of carboxylates (such as potassium, sodium, ammonium salts and triethanolammonium salts of higher fatty acids, etc.), sulfonates (such as sodium alkylbenzene sulfonate, α-olefin sulfonate (AOS), etc.), sulfates (fatty alcohol sulfates, secondary alkyl sulfates, etc.), phosphates (such as alkyl phosphate monoesters, diesters, etc.). In the present invention, the surface active emulsifier mainly functions by dispersing immiscible substances together to form tiny droplets, which are wrapped in the molecular layer of the surfactant to form an emulsion system.

[0010] Furthermore, the concentration of the ammonia water ranges from 15 to 25%.

[0011] Furthermore, the mesoporous nanomaterials include but are not limited to: one or more nanomaterials with mesoporous properties such as mesoporous nano-silicon dioxide and mesoporous nano-titanium dioxide. In the present invention, the mesoporous nanomaterials mainly function to load and slowly release ammonium stearate and delay the time point when ammonium stearate participates in the reaction.

[0012] Furthermore, the nanomaterials include but are not limited to: one or more of nano silicon dioxide, nano titanium dioxide, nano calcium carbonate, carbon nanotubes, and nano graphene. In the present invention, the functions of the nanomaterials include improving the pore structure of the silicon-aluminum gel material, improving the mechanical properties of the silicon-aluminum gel material, etc.

[0013] In a second aspect, the present invention discloses a process for preparing the first nano-modified ammonium stearate emulsion, comprising the following steps:

[0014] (1) The stearic acid, the surfactant emulsifier and water are mixed, and then the ammonia water is added dropwise under stirring to react. After the reaction is completed, the obtained reaction solution is subjected to mechanical shearing emulsification treatment to obtain an ammonium stearate emulsion, which is then used for standby use.

[0015] (2) adding the mesoporous nanomaterial to the ammonium stearate emulsion and mixing them evenly, and then loading the ammonium stearate into the mesoporous nanomaterial by a negative pressure loading method and combining them by van der Waals force, thereby obtaining the first nano-modified ammonium stearate emulsion.

[0016] Furthermore, in step (1), the stirring speed is 500 to 1000 rpm, and the reaction time is 12 to 15 hours.

[0017] Furthermore, in step (1), the rotation speed of the mechanical shearing emulsification treatment is 2000-2500 rpm, and the time range is 10-20 min.

[0018] Furthermore, in step (2), the negative pressure loading method comprises: adding the mixture of the mesoporous nano material and the ammonium stearate emulsion to a vacuum device, and then continuously vacuumizing the mixture, and then continuously introducing air after the vacuumizing is completed. Repeat the vacuumizing and introducing air steps several times to obtain the nano-modified ammonium stearate emulsion. Optionally, the continuous vacuumizing time is 20 to 40 minutes, and the continuous air introduction time is 10 to 20 minutes.

[0019] In a third aspect, the present invention discloses a process for preparing the second nano-modified ammonium stearate emulsion, comprising the steps of:

[0020] (S1) Adding the nanomaterial into the water to form a dispersion for later use.

[0021] (S2) adding the stearic acid and the surfactant emulsifier to the dispersion, then dropping ammonia water, and stirring the mixture under heating conditions to form an ammonium stearate liquid, and subjecting the liquid to mechanical shearing emulsification treatment to obtain the second nano-modified ammonium stearate emulsion.

[0022] Furthermore, in step (S1), the nanomaterial is added to the water and stirred at a rate of 500 to 600 rpm for 15 to 30 minutes.

[0023] Furthermore, in step (S2), the stirring speed is 800-1000 rpm, the stirring reaction time is 120-150 min, and the heating temperature is 70-80° C. In this step, stearic acid and ammonia water react under the action of a surfactant emulsifier to generate ammonium stearate liquid, and the nanomaterial is wrapped on the surface of the ammonium stearate to form a core-shell structure.

[0024] Furthermore, in step (S2), the rotation speed of the mechanical shearing emulsification treatment is 2000-2500 rpm, and the time is 30-45 min. In this step, the ammonium stearate liquid forms an emulsion system through shearing emulsification under the action of the surfactant emulsifier.

[0025] In a fourth aspect, the present invention discloses the use of the efflorescence inhibitor in a silica-alumina gelling material. Preferably, the method of the application comprises the steps of: adding the efflorescence inhibitor to a silica-alumina gelling material containing an alkali activator (such as sodium / potassium silicate, sodium / potassium hydroxide, etc.) and stirring evenly, and then firstly performing low-temperature curing at -10 to 0°C for 2 to 4 days. After completion, continue curing at 40 to 60°C for the 5th to 7th day, and finally perform natural curing to a set age.

[0026] Furthermore, the amount of the efflorescence inhibitor added is 2-5% of the mass of the silica-alumina gelling material.

[0027] Compared with the prior art, the present invention has at least the following beneficial technical effects:

[0028] As mentioned above, the traditional method of simply densifying or waterproofing the silica-alumina gel material to inhibit efflorescence has little effect and cannot maintain the long-term efflorescence inhibition effect. To this end, the present invention first provides a technical solution for curing the alkali metal cations in the silica-alumina gel material by using ammonium stearate loaded on the mesoporous nanomaterial and combined by van der Waals force. This is because: the ammonium stearate can react with the alkaline hydroxide in the silica-alumina gel material to form stearate, and these water-insoluble precipitates (such as sodium stearate and calcium stearate) construct a "maze effect", which can significantly prolong the difficulty of water-salt transmission, that is: the water-salt is constantly blocked when transmitting through the capillary in the hardened gel material, and then has to continuously select other capillary channels, thereby providing more sufficient time for the reaction of ammonium stearate with sodium ions and calcium ions, that is, after being blocked, it helps to promote more sodium ions and calcium ions to react with ammonium stearate, reduce the overflow of these ions, and thus inhibit the efflorescence phenomenon of the silica-alumina gel material. At the same time, the sodium stearate and calcium stearate as hydrophobic substances further improve the surface tension of the capillary pores in the silica-alumina gel material, greatly reducing the capillary effect. The above results can effectively reduce the diffusion rate of the alkali metal cations in the pore structure of the silica-alumina gel material, prevent leaching, and effectively inhibit the efflorescence phenomenon. In addition, the present invention also prepares a second nano-modified ammonium stearate emulsion, in which the nano-material can fill the micropores formed by the ammonia released when ammonium stearate reacts with sodium and calcium ions in the silica-alumina gel material, improve the pore structure of the silica-alumina gel material, and obtain a more compact structure, thereby significantly improving the anti-efflorescence ability and durability while ensuring the good mechanical properties of the aluminum gel material matrix.

[0029] Finally, the present invention also provides a special use method of the efflorescence inhibitor in the silica-alumina gelling material, namely: firstly, the alkali activator and the silica-alumina gelling material are subjected to low-temperature curing to form a gel to construct a strength structure. This is because the reaction between ammonium stearate and the alkali activator is an endothermic reaction. The reaction between the two can be effectively inhibited during the low-temperature curing stage, avoiding the consumption of the alkali activator by ammonium stearate, so that the construction of the strength structure can be completed more fully in advance. Then, high-temperature curing is performed to provide conditions for the reaction between ammonium stearate and the alkali activator remaining in the reaction, thereby consuming the remaining alkali activator and reducing the late efflorescence phenomenon caused by the alkaline substances remaining in the alkali activator. The above method can minimize the hydration inhibition effect of the ammonium stearate emulsion on the gelling component, thereby achieving the purpose of inhibiting efflorescence and maintaining strength at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. The embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein:

[0031] Figure 1 This is a diagram of the efflorescence effect of the test piece prepared in the following Example 1 when it is 28 days old.

[0032] Figure 2 This is a diagram of the efflorescence effect of the test piece prepared in the following Example 2 when it is 28 days old.

[0033] Figure 3 This is a diagram of the efflorescence effect of the test piece prepared in the following Example 3 when it is 28 days old.

[0034] Figure 4 This is a diagram of the efflorescence effect of the test piece prepared in the following Example 4 when it is 28 days old.

[0035] Figure 5 This is a diagram of the efflorescence effect of the test piece prepared in the following Example 5 when it is 28 days old.

[0036] Figure 6 This is a diagram of the efflorescence effect of the test piece prepared in the following Example 6 when it is 28 days old.

[0037] Figure 7 This is a diagram of the efflorescence effect of the test piece prepared in the following Example 7 when it is 28 days old.

[0038] Figure 8 This is a diagram of the efflorescence effect of the test piece prepared in the following Example 8 when it is 28 days old.

[0039] Fig. 9 This is a diagram of the efflorescence effect of the test piece prepared in the following Example 9 when it is 28 days old.

[0040] Fig.10 This is a diagram of the efflorescence effect of the test piece prepared in the following Example 10 when it is 28 days old. DETAILED DESCRIPTION

[0041] The present invention is further described below in conjunction with specific embodiments. These embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. The preferred implementation methods and materials described herein are only for demonstration purposes. The present invention is described in detail below in conjunction with specific implementation methods.

[0042] Example 1

[0043] (I) A process for preparing an efflorescence inhibitor, comprising the following steps:

[0044] 1. Preparation of the first nano-modified ammonium stearate emulsion:

[0045] (1) Prepare the following raw material components: 25 parts by weight of stearic acid, 2.6 parts by weight of sodium lauryl sulfate surfactant emulsifier, 23 parts by weight of 15% ammonia water, 0.2 parts by weight of mesoporous nano-silica, and 41 parts by weight of water.

[0046] (2) Add the stearic acid, the surfactant emulsifier and the water into the reaction kettle in sequence and stir evenly, then add the ammonia water dropwise while stirring (stirring speed 800 rpm) and react for 12 hours. After the reaction is completed, place the obtained reaction solution in an emulsifier and perform mechanical shearing emulsification treatment at a speed of 2300 rpm for 10 minutes to obtain an ammonium stearate emulsion for standby use.

[0047] (3) Add the mesoporous nano-silica to the ammonium stearate emulsion and stir magnetically for 2 hours, then add the obtained mixture to a vacuum drying oven and evacuate continuously for 30 minutes, and then continuously introduce air for 15 minutes. Repeat the above steps of evacuating and introducing air three times to obtain the first nano-modified ammonium stearate emulsion.

[0048] 2. Preparation of the second nano-modified ammonium stearate emulsion:

[0049] (S1) Prepare the following raw material components: 25 parts by weight of stearic acid, 2.6 parts by weight of sodium lauryl sulfate surfactant emulsifier, 23 parts by weight of ammonia water with a mass concentration of 15%, 0.2 parts by weight of nano-silicon dioxide, and 41 parts by weight of water.

[0050] (S2) adding the nano silicon dioxide to the water and stirring at a rate of 600 rpm for 15 minutes to form a dispersion. Adding the stearic acid, the surfactant emulsifier and the dispersion in turn into a reaction kettle, and then adding the ammonia water dropwise while stirring (stirring rate 800 rpm) for 120 minutes, the reaction temperature is 70° C., and then set aside.

[0051] (S3) placing the reaction solution obtained after the completion in an emulsifier for mechanical shearing emulsification treatment (shear rate 2000 rpm) for 30 minutes to obtain a second nano-modified ammonium stearate emulsion.

[0052] 3. The first nano-modified ammonium stearate emulsion and the second nano-modified ammonium stearate emulsion prepared in this example are mixed in a mass ratio of 1:1 and stirred evenly to obtain an efflorescence inhibitor.

[0053] (II) A process for preparing a silicon-alumina gelling material, comprising the following steps: preparing a silicon-alumina gelling material with the following components: 100 parts of slag, 10 parts of sodium silicate (alkali activator), 30 parts of water, and 0.5 parts of naphthalene-based high-efficiency water reducing agent. Then, 3% by weight of the efflorescence inhibitor prepared in this embodiment is added to the silicon-alumina gelling material. After stirring for 5 minutes, the obtained slurry is poured into a mold, and then first cured at -5°C for 3 days, and then cured at 55°C for the 7th day, and finally cured naturally for the 28th day to obtain the test piece.

[0054] Example 2

[0055] (I) A process for preparing an efflorescence inhibitor, comprising the following steps:

[0056] 1. Preparation of the first nano-modified ammonium stearate emulsion:

[0057] (1) Prepare the following raw material components: 30 parts by weight of stearic acid, 3 parts by weight of olefinoxysulfonate surfactant emulsifier, 25 parts by weight of 20% ammonia water, 0.25 parts by weight of mesoporous nano-titanium dioxide, and 45 parts by weight of water.

[0058] (2) Add the stearic acid, the surfactant emulsifier and the water into the reaction kettle in sequence and stir evenly, then add the ammonia water dropwise while stirring (stirring rate 1000 rpm) and react for 13 hours. After the reaction is completed, place the obtained reaction solution in an emulsifier and perform mechanical shearing emulsification treatment at a rate of 2000 rpm for 20 minutes to obtain an ammonium stearate emulsion for standby use.

[0059] (3) Add the mesoporous nano titanium dioxide to the ammonium stearate emulsion and stir magnetically for 2 hours, then add the obtained mixture to a vacuum drying oven and evacuate continuously for 40 minutes, and then continuously introduce air for 20 minutes. Repeat the above steps of evacuating and introducing air three times to obtain the first nano-modified ammonium stearate emulsion.

[0060] 2. Preparation of the second nano-modified ammonium stearate emulsion:

[0061] (S1) Prepare the following raw material components: 30 parts by weight of stearic acid, 3 parts by weight of olefinoxysulfonate surfactant emulsifier, 25 parts by weight of 20% ammonia water, 0.25 parts by weight of nano titanium dioxide, and 45 parts by weight of water.

[0062] (S2) adding the nano titanium dioxide to the water and stirring at a rate of 500 rpm for 30 minutes to form a dispersion. Adding the stearic acid, the surfactant emulsifier and the dispersion in the reaction kettle in sequence, and then adding the ammonia water dropwise while stirring (stirring rate 1000 rpm) to react for 140 minutes at a reaction temperature of 75° C. for standby use.

[0063] (S3) placing the reaction solution obtained after the completion in an emulsifier for mechanical shearing emulsification treatment (shear rate 2200 rpm) and homogenization time 40 min to obtain a second nano-modified ammonium stearate emulsion.

[0064] 3. The first nano-modified ammonium stearate emulsion and the second nano-modified ammonium stearate emulsion prepared in this example are mixed in a mass ratio of 1:2 and stirred evenly to obtain an efflorescence inhibitor.

[0065] (II) A process for preparing a silicon-alumina gelling material, comprising the following steps: preparing a silicon-alumina gelling material with the following components: 100 parts of slag, 10 parts of sodium silicate, 30 parts of water, and 0.5 parts of a naphthalene-based high-efficiency water reducer. Then, 5% by weight of the efflorescence inhibitor prepared in this embodiment is added to the silicon-alumina gelling material. After stirring for 5 minutes, the obtained slurry is poured into a mold, and then first cured at -10°C for 4 days, and then cured at 60°C for the 7th day, and finally cured naturally for the 28th day, to obtain a test piece.

[0066] Example 3

[0067] (I) A process for preparing an efflorescence inhibitor, comprising the following steps:

[0068] 1. Preparation of the first nano-modified ammonium stearate emulsion:

[0069] (1) Prepare the following raw material components: 20 parts by weight of stearic acid, 2 parts by weight of sodium secondary alkyl sulfonate surfactant emulsifier, 20 parts by weight of 25% ammonia water, 0.1 parts by weight of mesoporous nano-silica, and 35 parts by weight of water.

[0070] (2) Add the stearic acid, surfactant emulsifier and water into the reaction kettle in sequence and stir evenly, then add the ammonia water dropwise while stirring (stirring rate 500 rpm) and react for 15 hours. After the reaction is completed, place the obtained reaction solution in an emulsifier and perform mechanical shearing emulsification treatment at a rate of 2500 rpm for 15 minutes to obtain an ammonium stearate emulsion for standby use.

[0071] (3) Add the mesoporous nano-silica to the ammonium stearate emulsion and stir magnetically for 1.5 hours, then add the obtained mixture to a vacuum drying oven and evacuate continuously for 20 minutes, and then continue to introduce air for 10 minutes. Repeat the above steps of evacuating and introducing air for a total of five times to obtain the first nano-modified ammonium stearate emulsion.

[0072] 2. Preparation of the second nano-modified ammonium stearate emulsion:

[0073] (S1) Prepare the following raw material components: 20 parts by weight of stearic acid, 2 parts by weight of sodium secondary alkyl sulfonate surfactant emulsifier, 20 parts by weight of ammonia water with a mass concentration of 25%, 0.1 parts by weight of nano titanium dioxide, and 35 parts by weight of water.

[0074] (S2) adding the nano titanium dioxide to the water and stirring at a rate of 600 rpm for 25 minutes to form a dispersion. Adding the stearic acid, the surfactant emulsifier and the dispersion in the reaction kettle in sequence, and then adding the ammonia water dropwise while stirring (stirring rate 800 rpm) for 150 minutes, the reaction temperature is 80° C., and then set aside.

[0075] (S3) placing the reaction solution obtained after completion in an emulsifier for mechanical shearing emulsification treatment (shear rate 2500 rpm) and homogenization time 45 min to obtain a second nano-modified ammonium stearate emulsion.

[0076] 3. The first nano-modified ammonium stearate emulsion and the second nano-modified ammonium stearate emulsion prepared in this example are mixed in a mass ratio of 1:3 and stirred evenly to obtain an efflorescence inhibitor.

[0077] (II) A process for preparing a silicon-alumina gelling material, comprising the following steps: preparing a silicon-alumina gelling material with the following components: 100 parts of slag, 10 parts of sodium hydroxide, 30 parts of water, and 0.5 parts of a naphthalene-based high-efficiency water reducer. Then, 2% by weight of the efflorescence inhibitor prepared in this embodiment is added to the silicon-alumina gelling material. After stirring for 5 minutes, the obtained slurry is poured into a mold, and then first cured at 0°C for 2 days, and then cured at 40°C for the 5th day, and finally cured naturally for the 28th day to obtain a test piece.

[0078] Example 4

[0079] A preparation process of a silicon-alumina gelling material is the same as the above-mentioned Example 1, except that only the second nano-modified ammonium stearate emulsion prepared in the example is used as an efflorescence inhibitor. Specifically, the process comprises the following steps:

[0080] A silica-alumina gelling material with the following components was prepared: 100 parts of slag, 10 parts of sodium silicate, 30 parts of water, and 0.5 parts of naphthalene-based high-efficiency water reducing agent. Then, 3% by weight of the efflorescence inhibitor of Example 4 was added to the silica-alumina gelling material. After stirring for 5 minutes, the obtained slurry was poured into a mold, and then first cured at -5°C for 3 days, and then continued to be cured at 55°C until the 7th day, and finally naturally cured until the 28th day, and the test piece was obtained.

[0081] Example 5

[0082] A preparation process of a silica-alumina gelling material is the same as that of the above-mentioned embodiment 1, except that only the first nano-modified ammonium stearate emulsion prepared in the embodiment is used as an efflorescence inhibitor.

[0083] Specifically, the process includes the following steps: preparing a silicon-alumina gelling material with the following components: 100 parts of slag, 10 parts of sodium silicate, 30 parts of water, and 0.5 parts of naphthalene-based high-efficiency water reducer. Then, 3% by weight of the efflorescence inhibitor of Example 5 is added to the silicon-alumina gelling material. After stirring for 5 minutes, the obtained slurry is poured into a mold, and then firstly cured at -5°C for 3 days, and then continued to be cured at 55°C until the 7th day after completion, and finally naturally cured until the 28th day, and the test piece is obtained.

[0084] Example 6

[0085] (I) A preparation process of an efflorescence inhibitor is the same as that of the above-mentioned Example 2, except that the preparation of the first nano-modified ammonium stearate emulsion adopts the following steps:

[0086] (1) Prepare the following raw material components: 30 parts by weight of stearic acid, 3 parts by weight of an olefinoxysulfonate surfactant emulsifier, 25 parts by weight of 20% ammonia water, and 45 parts by weight of water.

[0087] (2) Add the stearic acid, the surfactant emulsifier and the water into the reaction kettle in sequence and stir evenly, then add the ammonia water dropwise while stirring (stirring rate 1000 rpm) and react for 13 hours. After the reaction is completed, place the obtained reaction solution in an emulsifier and perform mechanical shearing emulsification treatment at a rate of 2000 rpm for 20 minutes to obtain an ammonium stearate emulsion for standby use.

[0088] (3) Add the ammonium stearate emulsion into a vacuum drying oven and continuously evacuate for 40 minutes, then continuously introduce air for 20 minutes. Repeat the above evacuation and introduction of air three times to obtain the first nano-modified ammonium stearate emulsion.

[0089] (II) A process for preparing a silicon-alumina gelling material, comprising the following steps: preparing a silicon-alumina gelling material with the following components: 100 parts of slag, 10 parts of sodium silicate, 30 parts of water, and 0.5 parts of a naphthalene-based high-efficiency water reducer. Then, 5% by weight of the efflorescence inhibitor prepared in Example 6 is added to the silicon-alumina gelling material. After stirring for 5 minutes, the obtained slurry is poured into a mold, and then first cured at -10°C for 4 days, and then cured at 60°C for the 7th day, and finally cured naturally for the 28th day, to obtain a test piece.

[0090] Example 7

[0091] (I) A preparation process of an efflorescence inhibitor is the same as that of the above-mentioned Example 2, except that the preparation of the first nano-modified ammonium stearate emulsion adopts the following steps:

[0092] (1) Prepare the following raw material components: 20 parts by weight of commercially available ammonium stearate, 3 parts by weight of olefinoxysulfonate surfactant emulsifier, 0.25 parts by weight of mesoporous nano-titanium dioxide, and 45 parts by weight of water.

[0093] (2) The ammonium stearate and the surfactant emulsifier are placed in an emulsifier, and subjected to mechanical shearing emulsification treatment at a rate of 2000 rpm for 20 min to obtain an ammonium stearate emulsion for standby use.

[0094] (3) Add the mesoporous nano titanium dioxide to the ammonium stearate emulsion and stir magnetically for 2 hours, then add the obtained mixture to a vacuum drying oven and evacuate continuously for 40 minutes, and then continuously introduce air for 20 minutes. Repeat the above steps of evacuating and introducing air three times to obtain the first nano-modified ammonium stearate emulsion.

[0095] (4) The first nano-modified ammonium stearate emulsion prepared in this example and the second nano-modified ammonium stearate emulsion prepared by the method of Example 2 were mixed in a mass ratio of 1:2 and stirred evenly to obtain an efflorescence inhibitor.

[0096] (II) A process for preparing a silicon-alumina gelling material, comprising the following steps: preparing a silicon-alumina gelling material with the following components: 100 parts of slag, 10 parts of sodium silicate, 30 parts of water, and 0.5 parts of a naphthalene-based high-efficiency water reducer. Then, 5% by weight of the efflorescence inhibitor prepared in Example 7 is added to the silicon-alumina gelling material. After stirring for 5 minutes, the obtained slurry is poured into a mold, and then first cured at -10°C for 4 days, and then cured at 60°C for the 7th day, and finally cured naturally for the 28th day, to obtain a test piece.

[0097] Example 8

[0098] (I) A preparation process of an efflorescence inhibitor is the same as that of the above-mentioned Example 3, except that the preparation of the second nano-modified ammonium stearate emulsion adopts the following steps:

[0099] (S1) Prepare the following raw material components: 20 parts by weight of commercially available ammonium stearate, 2 parts by weight of a secondary alkyl sulfonate surfactant emulsifier, 0.1 parts by weight of nano titanium dioxide, and 35 parts by weight of water.

[0100] (S2) adding the nano titanium dioxide to the water and stirring at a rate of 600 rpm for 25 min to form a dispersion. In a reaction kettle, the ammonium stearate and the surface active emulsifier are sequentially added to the dispersion and mixed evenly, and then the obtained mixture is placed in an emulsifier for mechanical shearing emulsification treatment (shear rate 2500 rpm) for 45 min to obtain a second nano modified ammonium stearate emulsion.

[0101] (S3) The second nano-modified ammonium stearate emulsion prepared in this example and the first nano-modified ammonium stearate emulsion prepared by the method of Example 3 are mixed in a mass ratio of 1:3 and stirred evenly to obtain an efflorescence inhibitor.

[0102] (II) A process for preparing a silicon-alumina gelling material, comprising the following steps: preparing a silicon-alumina gelling material with the following components: 100 parts of slag, 10 parts of sodium hydroxide, 30 parts of water, and 0.5 parts of a naphthalene-based high-efficiency water reducer. Then, 2% by weight of the efflorescence inhibitor prepared in Example 8 is added to the silicon-alumina gelling material. After stirring for 5 minutes, the obtained slurry is poured into a mold, and then first cured at 0°C for 2 days, and then cured at 40°C for the 5th day, and finally cured naturally for the 28th day to obtain a test piece.

[0103] Example 9

[0104] A preparation process of a silicon-alumina gelling material comprises the following steps: preparing a silicon-alumina gelling material with the following components: 100 parts of slag, 10 parts of sodium hydroxide, 30 parts of water, and 0.5 parts of a naphthalene-based high-efficiency water reducer. Then, 2% by weight of the efflorescence inhibitor prepared in Example 3 is added to the silicon-alumina gelling material. After stirring for 5 minutes, the obtained slurry is poured into a mold, and then heat-cured at 40° C. for 5 days, and finally naturally cured for 28 days to obtain a test piece.

[0105] Example 10

[0106] A preparation process of a silicon-alumina gelling material comprises the following steps: preparing a silicon-alumina gelling material with the following components: 100 parts of slag, 10 parts of sodium silicate, 30 parts of water, and 0.5 parts of a naphthalene-based high-efficiency water reducer. Then, 3% by weight of the efflorescence inhibitor prepared in Example 1 is added to the silicon-alumina gelling material. After stirring for 5 minutes, the obtained slurry is poured into a mold, and then cured under standard conditions (temperature of 20±2°C and relative humidity of 95±5%RH) until the 28th day to obtain a test piece.

[0107] The performance indicators of the test pieces prepared in the above embodiments were tested, wherein: the alkali ion overflow concentration is to soak the sealed and cured sample in 200 ml ultrapure water for 30 minutes, and then use an ultrasonic cleaner to clean it for 10 minutes, take 10 ml of the solution, and use ICP-OES to determine the ion concentration of the leachate. The compressive strength is to pour the silicon-aluminum gelling material slurry into a mold with a size of 2mm×2mm×2mm, and then cover the surface of the sample with a plastic film for 24 hours, then take out the sample and demold it. The demolded sample is cured to the specified age, and the compressive strength is tested using a universal testing machine (MTS, CMT5504). The overflow mass ratio of weathering products is to weigh the sample that has been cured to the age, and then scrape off the surface weathering products and weigh them. The mass ratio of the sample to the sample is the overflow mass ratio of weathering products. Capillary water absorption is to mold the sample into a cylindrical (Ф50×50mm) mold, treat it with epoxy resin after drying, so that the sides and bottom of the sample are completely covered, and then immerse the uncovered surface in water about 0.5mm high for capillary water absorption test until the weight is constant. The specific calculation formula is as follows:

[0108]

[0109] In the above formula, W is the water absorption rate of the sample (%), M1 is the wet mass of the sample at different times (g), and M0 is the initial mass of the sample after drying (g).

[0110] The test results of the above-mentioned alkali ion overflow concentration, compressive strength, weathering product overflow mass ratio and capillary water absorption are shown in the following table:

[0111]

[0112]

[0113] In addition, if Figures 1 to 10 As shown, they are respectively the efflorescence effect diagrams of the test pieces prepared in Examples 1 to 10 when they are 28 days old. It can be seen that the ability of the test pieces in Examples 1 to 3 to resist efflorescence is significantly better than that of other examples.

[0114] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A pyrolyzing inhibitor, characterized in that The invention comprises two nano-modified ammonium stearate emulsions; wherein: the first nano-modified ammonium stearate emulsion is an emulsion formed by ammonium stearate loaded on a mesoporous nano-material and combined by van der Waals force; the second nano-modified ammonium stearate emulsion is an emulsion system formed by ammonium stearate with a surface coated with nano-particle material dispersed in an emulsion; the mass ratio of the first nano-modified ammonium stearate emulsion to the second nano-modified ammonium stearate emulsion is 1:1-3; The raw material composition of the first nano-modified ammonium stearate emulsion includes: 20-30 parts by weight of stearic acid, 2-3 parts by weight of surfactant emulsifier, 20-25 parts by weight of ammonia water, 0.1-0.25 parts by weight of mesoporous nanomaterial, and 35-45 parts by weight of water; The raw material composition of the second nano-modified ammonium stearate emulsion includes: 20-30 parts by weight of stearic acid, 2-3 parts by weight of surfactant emulsifier, 20-25 parts by weight of ammonia water, 0.1-0.25 parts by weight of nano-material, and 35-45 parts by weight of water; The preparation process of the first nano-modified ammonium stearate emulsion comprises the following steps: (1) mixing the stearic acid, the surfactant emulsifier and water, and then adding the ammonia water dropwise under stirring to react. After the reaction is completed, the obtained reaction solution is subjected to mechanical shearing emulsification treatment to obtain an ammonium stearate emulsion for standby use; (2) adding the mesoporous nanomaterial to the ammonium stearate emulsion and mixing them evenly, and then loading the ammonium stearate into the mesoporous nanomaterial by a negative pressure loading method and combining them by van der Waals force, thereby obtaining the first nano-modified ammonium stearate emulsion; The preparation process of the second nano-modified ammonium stearate emulsion comprises the following steps: (S1) adding the nanomaterial into the water to form a dispersion for later use; (S2) adding the stearic acid and the surfactant emulsifier to the dispersion, then dropping ammonia water, and stirring under heating conditions to react to form an ammonium stearate liquid, and subjecting the liquid to mechanical shearing emulsification treatment to obtain the second nano-modified ammonium stearate emulsion.

2. The efflorescence inhibitor according to claim 1, characterized in that The mesoporous nanomaterials include: one or more of mesoporous nano-silicon dioxide and mesoporous nano-titanium dioxide.

3. The efflorescence inhibitor according to claim 1, characterized in that The nanomaterials include: one or more of nano silicon dioxide, nano titanium dioxide, nano calcium carbonate, carbon nanotubes, and nano graphene.

4. The efflorescence inhibitor according to claim 1, characterized in that The surface active emulsifier includes at least one of carboxylates, sulfonates, sulfates and phosphates.

5. The efflorescence inhibitor according to claim 1, characterized in that The concentration range of the ammonia water is 15-25%.

6. The efflorescence inhibitor according to claim 1, characterized in that In step (1), the stirring speed is 500-1000 rpm, and the reaction time is 12-15 h.

7. The efflorescence inhibitor according to claim 1, characterized in that In step (1), the rotation speed of the mechanical shearing emulsification treatment is 2000-2500 rpm, and the time range is 10-20 min.

8. The efflorescence inhibitor according to claim 1, characterized in that In step (2), the negative pressure loading method comprises: adding the mixture of the mesoporous nanomaterial and the ammonium stearate emulsion into a vacuum device, and then continuously evacuating the mixture, and then continuously introducing air after the evacuation; repeating the evacuation and introducing air steps several times to obtain the nano-modified ammonium stearate emulsion.

9. The efflorescence inhibitor according to claim 8, characterized in that The continuous vacuuming time is 20 to 40 minutes, and the continuous air introduction time is 10 to 20 minutes.

10. The efflorescence inhibitor according to claim 1, characterized in that In step (S1), the nanomaterial is added to the water and then stirred at a speed of 500-600 rpm for 15-30 min.

11. The efflorescence inhibitor according to claim 1, characterized in that In step (S2), the stirring speed is 800-1000 rpm, the stirring reaction time is 120-150 min, and the heating temperature is 70-80°C.

12. The efflorescence inhibitor according to claim 1, characterized in that In step (S2), the rotation speed of the mechanical shearing emulsification treatment is 2000-2500 rpm, and the time is 30-45 min.

13. Use of the efflorescence inhibitor according to any one of claims 1 to 12 in silica-alumina gelling materials.

14. The use according to claim 13, characterized in that The application method comprises the steps of: adding the efflorescence inhibitor into the silica-alumina gelling material containing the alkali activator and stirring evenly, and then firstly performing low-temperature curing at -10 to 0°C for 2 to 4 days; after completion, continuing curing at 40 to 60°C for the 5th to 7th day, and finally performing natural curing to the set age.

15. The use according to claim 13, characterized in that: The amount of the efflorescence inhibitor added is 2-5% of the mass of the silica-alumina gelling material.