A method for preparing a tundish retaining wall using recycled materials
Through the proportion and process design of alumina-magnesia-carbon brick recycled materials without hydration treatment, the problems of resource waste and environmental pollution in the preparation of alumina-magnesia-carbon brick recycled materials are solved, and the efficient preparation and cost reduction of the tundish retaining wall are achieved.
Patent Information
- Application Number
- CN202310567840.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-05-19
AI Technical Summary
In the existing technology, alumina-magnesia carbon brick recycled materials need to undergo a long-term hydration treatment, resulting in resource waste and environmental pollution. At the same time, the preparation efficiency is low and the production cost is increased.
The tundish retaining wall is prepared by using alumina-magnesia-carbon brick recycled material without hydration treatment, through a reasonable proportion of recycled alumina-magnesia-carbon brick waste, magnesia, silica powder and α-alumina powder, combined with forming, curing and drying processes. , avoid the hydration step.
It realizes the efficient utilization of alumina-magnesia carbon brick recycled materials, reduces product costs and environmental pressure, improves preparation efficiency, and ensures the fire-resistant performance of the product.
Abstract
Description
Technical Field
[0001] The invention relates to refractory material technology, in particular to recycled refractory material, and specifically to a method for preparing a tundish retaining wall by using recycled material. Background Art
[0002] The tundish is an indispensable container for storing and distributing molten steel between the ladle and the crystallizer in the continuous casting process. With the development of ultra-clean steel and defect-free ingot production, the requirements for the cleanliness of the continuous casting molten steel are getting higher and higher. Especially under the promotion of efficient continuous casting technology, the casting speed of the continuous casting machine is getting higher and higher, and the non-metallic inclusions in the molten steel enter the crystallizer and solidify before they can float up. Therefore, in the process of development of tundish metallurgy, various types of flow control devices have been formed, such as slag dams, slag weirs, turbulence controllers, etc., and most of them use alkaline magnesium materials.
[0003] With the increase in environmental protection efforts, the price of raw materials has risen rapidly, and enterprises are facing huge production costs and operating pressures. In order to reduce the cost of refractory products, the recycling and reuse of waste products has become the preferred consideration. At present, the recycled aluminum-magnesium-carbon bricks are mostly used in ladle bricks, and their utilization in castables is relatively low. Moreover, according to the existing application technology of aluminum-magnesium-carbon brick recycled materials, aluminum-magnesium-carbon brick recycled materials must be fully hydrated (hydration time is usually greater than 72 hours) and dried, and cannot be used directly. Otherwise, the untreated recycled materials will react with water and cause problems such as bulges or hollows on the brick body. However, the hydration treatment time is long, which not only wastes a lot of water resources, but also seriously restricts the preparation efficiency of recycled materials. In addition, the chemical gases and precipitates produced by hydration decomposition will also cause environmental pollution. Summary of the invention
[0004] In response to the problems raised in the background technology, the purpose of the present invention is to provide a method for preparing a tundish retaining wall using recycled materials. Through reasonable process design, the tundish retaining wall can be directly made from recycled aluminum-magnesium-carbon bricks that have not been hydrated, thereby solving the efficiency and pollution problems in the preparation of products from recycled aluminum-magnesium-carbon bricks, reducing the application cost of recycled materials and improving enterprise benefits.
[0005] To achieve the above object, the present invention adopts the following technical solutions:
[0006] A method for preparing a tundish retaining wall using recycled materials comprises the following steps:
[0007] Step S1, preparing raw materials; the raw materials are calculated by weight, including 75-85 parts of recycled aluminum-magnesium-carbon brick waste, 15-30 parts of magnesia sand, 2-5 parts of 92 silicon micropowder, 1-3 parts of α-alumina micropowder, and 0.2-4 parts of additives; the magnesium oxide content in the recycled aluminum-magnesium-carbon brick waste is greater than 70%;
[0008] Step S2, mixing the recycled aluminum-magnesia-carbon brick waste, magnesia sand, silicon powder, α-alumina powder and additives to obtain a recycled tundish prefabricated castable;
[0009] Step S3, forming, curing and drying the regenerated tundish prefabricated castable obtained in step S2 to obtain a tundish prefabricated product; the specific steps are as follows:
[0010] S3.1, molding, put the recycled tundish prefabricated casting material into a mixer, add water and stir for 5 minutes, slowly put it into the mold, and turn on the vibration motor for 3 minutes to shape the embryo in the mold;
[0011] Step S3.2, curing, placing the embryo body and the mold together in a curing kiln for curing for 24 hours at a curing temperature of 70°C and a humidity of 60%, and then demolding to obtain a semi-finished product; the curing kiln is provided with a spray device, which is used to control the humidity and dilute the ammonia released during the embryo body curing process;
[0012] Step S3.3, drying, drying the semi-finished product at a drying temperature of 350° C. for 70 hours to obtain a tundish retaining wall product.
[0013] In the step S1, the recycled aluminum-magnesium-carbon brick waste is composed of the following components: 10-30 parts of recycled aluminum-magnesium-carbon brick waste with a particle size of 8-15mm, 10-25 parts of recycled aluminum-magnesium-carbon brick waste with a particle size of 5-8mm, 10-20 parts of recycled aluminum-magnesium-carbon brick waste with a particle size of 3-5mm, and 10-20 parts of recycled aluminum-magnesium-carbon brick waste with a particle size of 1-3mm.
[0014] In the step S1, the recycled aluminum-magnesium-carbon brick waste is obtained according to the following method: the steel slag and scrap steel on the surface of the used aluminum-magnesium-carbon waste bricks are cleaned to obtain the required aluminum-magnesium-carbon brick waste chunks, and then the aluminum-magnesium-carbon brick chunks are crushed to the required particle size, and iron removal is performed while crushing to finally obtain recycled aluminum-magnesium-carbon brick waste.
[0015] In the step S1, the magnesia is composed of 0-1 mm magnesia particles and 200 mesh magnesia fine powder according to the following mass ratio: 10-18 parts of 0-1 mm magnesia particles and 15-20 parts of 200 mesh magnesia fine powder; the magnesium oxide content in the magnesia is greater than 95%.
[0016] In the step S1, the particle size of the silicon micropowder is 5-10 μm, and the silicon dioxide content in the silicon micropowder is greater than 92%.
[0017] In the step S1, the particle size of the a-alumina powder is 1-3 μm, and the alumina content is >99.5%.
[0018] In the step S2, the additive is stainless steel fiber, organic fiber, sodium hexametaphosphate or sodium tripolyphosphate.
[0019] Compared with the prior art, the present invention has the following advantages:
[0020] The recycled material tundish retaining wall of the present invention adopts recycled aluminum-magnesium-carbon brick waste as the main raw material. Through the reasonable selection of the particle size of the recycled aluminum-magnesium-carbon brick waste and the limitation of the magnesium oxide content, the magnesium oxide content in the recycled aluminum-magnesium-carbon brick waste is greater than 70%, thereby preventing the product from having low refractoriness due to too low magnesium content and excessive spinel phase generated at high temperature, which affects the product's anti-corrosion and anti-scouring properties.
[0021] The present invention breaks through the existing technical barriers and enables the crushed granular materials of recycled aluminum-magnesium-carbon brick waste to be used directly without hydration treatment. The product surface has no bulges or faults, which greatly reduces the manufacturing cost and environmental pressure of recycled raw materials. Implementation
[0022] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] The present invention provides a method for preparing a tundish retaining wall using recycled materials, comprising the following steps:
[0024] Step S1, preparing raw materials; the raw materials are calculated by weight, including 75-85 parts of recycled aluminum-magnesium-carbon brick waste, 15-30 parts of magnesia sand, 2-5 parts of 92 silicon micropowder, 1-3 parts of α-alumina micropowder, and 0.2-4 parts of additives; the magnesium oxide content in the recycled aluminum-magnesium-carbon brick waste is greater than 70%;
[0025] Step S2, mixing the recycled aluminum-magnesia-carbon brick waste, magnesia sand, silicon powder, α-alumina powder and additives to obtain a recycled tundish prefabricated castable;
[0026] Step S3, forming, curing and drying the regenerated tundish prefabricated castable obtained in step S2 to obtain a tundish prefabricated product; the specific steps are as follows:
[0027] S3.1, molding, put the recycled tundish prefabricated casting material into a mixer, add water and stir for 5 minutes, slowly put it into the mold, and turn on the vibration motor for 3 minutes to shape the embryo in the mold;
[0028] Step S3.2, curing, placing the embryo body and the mold together in a curing kiln for curing for 24 hours at a curing temperature of 70°C and a humidity of 60%, and then demolding to obtain a semi-finished product; the curing kiln is provided with a spray device, which is used to control the humidity and dilute the ammonia released during the embryo body curing process;
[0029] Step S3.3, drying, drying the semi-finished product at a drying temperature of 350° C. for 70 hours to obtain a tundish retaining wall product.
[0030] In the step S1, the recycled aluminum-magnesium-carbon brick waste is composed of the following components: 10-30 parts of recycled aluminum-magnesium-carbon brick waste with a particle size of 8-15mm, 10-25 parts of recycled aluminum-magnesium-carbon brick waste with a particle size of 5-8mm, 10-20 parts of recycled aluminum-magnesium-carbon brick waste with a particle size of 3-5mm, and 10-20 parts of recycled aluminum-magnesium-carbon brick waste with a particle size of 1-3mm.
[0031] In the step S1, the recycled aluminum-magnesium-carbon brick waste is obtained according to the following method: the steel slag and scrap steel on the surface of the used aluminum-magnesium-carbon waste bricks are cleaned to obtain the required aluminum-magnesium-carbon brick waste chunks, and then the aluminum-magnesium-carbon brick chunks are crushed to the required particle size, and iron removal is performed while crushing to finally obtain recycled aluminum-magnesium-carbon brick waste.
[0032] In the step S1, the magnesia is composed of 0-1 mm magnesia particles and 200 mesh magnesia fine powder according to the following mass ratio: 10-18 parts of 0-1 mm magnesia particles and 15-20 parts of 200 mesh magnesia fine powder; the magnesium oxide content in the magnesia is greater than 95%.
[0033] In the step S1, the particle size of the silicon micropowder is 5-10 μm, and the silicon dioxide content in the silicon micropowder is greater than 92%.
[0034] In the step S1, the particle size of the a-alumina powder is 1-3 μm, and the alumina content is >99.5%.
[0035] In the step S2, the additive is stainless steel fiber, organic fiber, sodium hexametaphosphate or sodium tripolyphosphate.
[0036] The recycled aluminum-magnesium-carbon brick waste used in the present invention mainly comes from the ladle. The residual bricks in the ladle must be completely removed when the thickness reaches the lower limit of safe use. The residual bricks that do not contact the molten steel can be recycled and can replace the magnesia sand used in the original ladle retaining wall after selection and crushing. The cost of the recycled waste aluminum-magnesium-carbon bricks is 1 / 2 of the price of magnesia sand, which greatly reduces the cost of retaining wall products.
[0037] The main functions of adding 0-1 mm magnesia particles and 200 mesh magnesia fine powder in the present invention are: the 0-1 mm magnesia particles fill the gaps in the skeleton structure, and the 200 mesh magnesia fine powder as a matrix is conducive to improving the strength at room temperature.
[0038] In the present invention, the addition of silicon micropowder mainly serves to fill the pores of the refractory castable, thereby making the internal structure of the retaining wall tighter and improving the medium and high temperature strength.
[0039] In the present invention, the addition of α-alumina powder is mainly beneficial to improving the rheology and sintering properties of the castable and increasing the strength of the castable. Example
[0040] The preparation process of the tundish retaining wall is briefly described as follows:
[0041] First, clean the steel slag and scrap steel on the surface of the used aluminum-magnesium carbon bricks to obtain the required aluminum-magnesium carbon brick waste blocks, and then crush the aluminum-magnesium carbon brick blocks to the required particle size, and remove iron while crushing to obtain recycled aluminum-magnesium carbon brick waste; the recycled aluminum-magnesium carbon brick waste includes: 10 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 8-15mm, 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 5-8mm, 20 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 3-5mm, and 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 1-3mm; the magnesium oxide content in the recycled aluminum-magnesium carbon brick waste is greater than 70%;
[0042] Select 16 parts of 0-1mm magnesia particles, 0.1 parts of organic fiber, and 1.2 parts of steel fiber and mix for 2 minutes, add 18 parts of 200 mesh magnesia fine powder, 3 parts of silicon powder, 3 parts of α-alumina powder with a particle size of 3μm, and 0.2 parts of sodium hexametaphosphate and continue mixing for 5 minutes to obtain a regenerated tundish prefabricated castable;
[0043] Put the recycled tundish prefabricated castable into a mixer, add water and stir for 5 minutes, slowly put it into the mold, turn on the vibration motor for 3 minutes, put the mold and the embryo into a curing kiln for curing for 24 hours (temperature 70℃, humidity 60%), and dry the semi-finished product after demoulding at 350℃*70h to obtain the finished tundish retaining wall.
[0044] In Example 1, the magnesium oxide content in the magnesia is >95%; the particle size of the silicon micropowder is 5-10 μm, and the silicon dioxide content in the silicon micropowder is >92%; the particle size of the α-alumina micropowder is 1-3 μm, and the aluminum oxide content is >99.5%.
[0045] The main physical and chemical indicators of sample 1 obtained in the embodiment are as follows: Mg ≥ 70%, Al2O3 ≥ 10%; the bulk density after baking at 110°C is ≥ 2.65 g / cm 3 The apparent porosity is ≤16.0%, the compressive strength (110℃×24h) is 38.0MPa, and the high temperature flexural strength (1400×0.3h) is 1.25MPa; Sample 1 was used on a double-flow slab middle package of a steel plant for 16 hours. After it was offline, the slag line of the retaining wall was corroded by 15mm, meeting the use requirements of the steel plant. Example
[0046] The preparation process of the tundish retaining wall is briefly described as follows:
[0047] Clean the steel slag and scrap steel on the surface of the used aluminum-magnesium carbon bricks to obtain the required aluminum-magnesium carbon brick waste blocks, and then crush the aluminum-magnesium carbon brick blocks to the required particle size, and remove iron while crushing to obtain recycled aluminum-magnesium carbon brick waste; the recycled aluminum-magnesium carbon brick waste includes: 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 8-15mm, 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 5-8mm, 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 3-5mm, and 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 1-3mm; the magnesium oxide content in the recycled aluminum-magnesium carbon brick waste is greater than 70%;
[0048] Select 16 parts of 0-1mm magnesia particles, 0.1 parts of organic fiber, and 1.2 parts of steel fiber and mix for 2 minutes, add 18 parts of 200 mesh magnesia fine powder, 3 parts of silicon powder, 3 parts of α-alumina powder with a particle size of 3μm, and 0.2 parts of sodium hexametaphosphate and continue mixing for 5 minutes to obtain a regenerated tundish prefabricated castable;
[0049] The recycled tundish prefabricated castable is placed in a mixer, water is added and stirred for 5 minutes, and then slowly placed in a mold. Meanwhile, the vibration motor is turned on for 3 minutes. The mold and the embryo are placed in a curing kiln for curing for 24 hours (temperature 70°C, humidity 60%). The semi-finished product after demoulding is dried at 350°C*70h to obtain a finished tundish retaining wall.
[0050] In Example 2, the magnesium oxide content in the magnesia is >95%; the particle size of the silicon micropowder is 5-10 μm, and the silicon dioxide content in the silicon micropowder is >92%; the particle size of the α-alumina micropowder is 1-3 μm, and the aluminum oxide content is >99.5%.
[0051] In the sample 2 obtained in Example 2, the main physical and chemical indicators are as follows: Mg ≥ 70%, Al2O3 ≥ 10%; the bulk density after baking at 110°C is ≥ 2.65 g / cm 3 The apparent porosity is ≤16.0%, the compressive strength (110℃×24h) is 39.2MPa, and the high temperature flexural strength (1400×0.3h) is 1.3MPa; Sample 2 was used on a double-flow slab middle package of a steel plant for 16 hours. After it was offline, the slag line of the retaining wall was corroded by 15mm, meeting the use requirements of the steel plant. Example
[0052] The preparation process of the tundish retaining wall is briefly described as follows:
[0053] Clean the steel slag and scrap steel on the surface of the used aluminum-magnesium carbon bricks to obtain the required aluminum-magnesium carbon brick waste blocks, and then crush the aluminum-magnesium carbon brick blocks to the required particle size, and remove iron while crushing to obtain recycled aluminum-magnesium carbon brick waste; the recycled aluminum-magnesium carbon brick waste includes: 12 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 8-15mm, 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 5-8mm, 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 3-5mm, and 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 1-3mm; the magnesium oxide content in the recycled aluminum-magnesium carbon brick waste is greater than 70%;
[0054] Select 16 parts of 0-1mm magnesia particles, 0.1 parts of organic fiber, and 1.2 parts of steel fiber and mix for 2 minutes, add 20 parts of 200 mesh magnesia fine powder, 3.5 parts of silicon powder, 2.5 parts of α-alumina powder with a particle size of 3μm, and 0.2 parts of sodium hexametaphosphate and continue mixing for 5 minutes to obtain a regenerated tundish prefabricated castable;
[0055] The recycled tundish prefabricated castable is placed in a mixer, water is added and stirred for 5 minutes, and then slowly placed in a mold. Meanwhile, the vibration motor is turned on for 3 minutes. The mold and the embryo are placed in a curing kiln for curing for 24 hours (temperature 70°C, humidity 60%). The semi-finished product after demoulding is dried at 350°C*70h to obtain a finished tundish retaining wall.
[0056] In Example 3, the magnesium oxide content in the magnesia is >95%; the particle size of the silicon micropowder is 5-10 μm, and the silicon dioxide content in the silicon micropowder is >92%; the particle size of the α-alumina micropowder is 1-3 μm, and the aluminum oxide content is >99.5%.
[0057] The main physical and chemical indicators of sample 3 obtained in Example 3 are as follows: Mg ≥ 70%, Al2O3 ≥ 10%; the bulk density after baking at 110°C is ≥ 2.65 g / cm 3 The apparent porosity is ≤16.0%, the compressive strength (110℃×24h) is 41.3MPa, and the high temperature flexural strength (1400×0.3h) is 1.3MPa; Sample 3 was used on a double-flow slab middle package of a steel plant for 16 hours. After it was offline, the slag line of the retaining wall was corroded by 15mm, meeting the use requirements of the steel plant. Example
[0058] The preparation process of the tundish retaining wall is briefly described as follows:
[0059] Clean the steel slag and scrap steel on the surface of the used aluminum-magnesium carbon bricks to obtain the required aluminum-magnesium carbon brick waste blocks, and then crush the aluminum-magnesium carbon brick blocks to the required particle size, and remove iron while crushing to obtain recycled aluminum-magnesium carbon brick waste; the recycled aluminum-magnesium carbon brick waste includes: 13 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 8-15mm, 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 5-8mm, 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 3-5mm, and 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 1-3mm; the magnesium oxide content in the recycled aluminum-magnesium carbon brick waste is greater than 70%;
[0060] Select 16 parts of 0-1mm magnesia particles, 0.15 parts of organic fiber, and 1 part of steel fiber and mix them for 2 minutes, then add 19 parts of 200-mesh magnesia fine powder, 3.5 parts of silicon powder, 2.5 parts of α-alumina powder with a particle size of 3 μm, and 0.2 parts of sodium hexametaphosphate and continue mixing for 5 minutes to obtain a regenerated tundish prefabricated castable;
[0061] The recycled tundish prefabricated castable is placed in a mixer, water is added and stirred for 5 minutes, and then slowly placed in a mold. Meanwhile, the vibration motor is turned on for 3 minutes, and the mold and the embryo are placed in a curing kiln for curing for 24 hours (temperature 70°C, humidity 60%). The semi-finished product after demoulding is dried at 350°C*70h to obtain a finished tundish retaining wall.
[0062] In Example 4, the magnesium oxide content in the magnesia is >95%; the particle size of the silicon micropowder is 5-10 μm, and the silicon dioxide content in the silicon micropowder is >92%; the particle size of the α-alumina micropowder is 1-3 μm, and the aluminum oxide content is >99.5%; the additives are stainless steel fiber, organic fiber, and sodium hexametaphosphate.
[0063] The main physical and chemical indicators of sample 4 obtained in Example 4 are as follows: Mg ≥ 70%, Al2O3 ≥ 10%; the bulk density after baking at 110°C is ≥ 2.65 g / cm 3 The apparent porosity is ≤16.0%, the compressive strength (110℃×24h) is 41.5MPa, and the high temperature flexural strength (1400×0.3h) is 1.3MPa; Sample 4 was used for 16 hours on a double-flow slab middle package of a steel plant. After it was offline, the slag line of the retaining wall was corroded by 15mm, meeting the use requirements of the steel plant. Example
[0064] The preparation process of the tundish retaining wall is briefly described as follows:
[0065] Clean the steel slag and scrap steel on the surface of the used aluminum-magnesium carbon bricks to obtain the required aluminum-magnesium carbon brick waste blocks, and then crush the aluminum-magnesium carbon brick blocks to the required particle size, and remove iron while crushing to obtain recycled aluminum-magnesium carbon brick waste; the recycled aluminum-magnesium carbon brick waste includes: 12 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 8-15mm, 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 5-8mm, 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 3-5mm, and 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 1-3mm; the magnesium oxide content in the recycled aluminum-magnesium carbon brick waste is greater than 70%;
[0066] Select 16 parts of 0-1mm magnesia particles, 0.2 parts of organic fiber, and 1 part of steel fiber and mix them for 2 minutes, then add 19 parts of 200-mesh magnesia fine powder, 4 parts of silicon powder, 2 parts of α-alumina powder with a particle size of 3 μm, and 0.15 parts of sodium hexametaphosphate and continue mixing for 5 minutes to obtain a regenerated tundish prefabricated castable;
[0067] The recycled tundish prefabricated castable is placed in a mixer, water is added and stirred for 5 minutes, and then slowly placed in a mold. Meanwhile, the vibration motor is turned on for 3 minutes. The mold and the embryo are placed in a curing kiln for curing for 24 hours (temperature 70°C, humidity 60%). The semi-finished product after demoulding is dried at 350°C*70h to obtain a finished tundish retaining wall.
[0068] In Example 5, the magnesium oxide content in the magnesia is >95%; the particle size of the silicon micropowder is 5-10 μm, and the silicon dioxide content in the silicon micropowder is >92%; the particle size of the α-alumina micropowder is 1-3 μm, and the aluminum oxide content is >99.5%; the additives are stainless steel fiber, organic fiber, and sodium hexametaphosphate.
[0069] In the sample 5 obtained in Example 5, the main physical and chemical indicators are as follows: Mg ≥ 70%, Al2O3 ≥ 10%; the bulk density after baking at 110°C is ≥ 2.65 g / cm 3 The apparent porosity is ≤16.0%, the compressive strength (110℃×24h) is 42.8MPa, and the high temperature flexural strength (1400×0.3h) is 1.32MPa; Sample 5 was used on a double-flow slab middle package of a steel plant for 16 hours. After it was offline, the slag line of the retaining wall was corroded by 15mm, meeting the use requirements of the steel plant. Example
[0070] The preparation process of the tundish retaining wall is briefly described as follows:
[0071] Clean the steel slag and scrap steel on the surface of the used aluminum-magnesium carbon bricks to obtain the required aluminum-magnesium carbon brick waste blocks, and then crush the aluminum-magnesium carbon brick blocks to the required particle size, and remove iron while crushing to obtain recycled aluminum-magnesium carbon brick waste; the recycled aluminum-magnesium carbon brick waste includes: 13 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 8-15mm, 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 5-8mm, 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 3-5mm, and 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 1-3mm; the magnesium oxide content in the recycled aluminum-magnesium carbon brick waste is greater than 70%;
[0072] Select 16 parts of 0-1mm magnesia particles, 0.2 parts of organic fiber, and 0.8 parts of steel fiber and mix for 2 minutes, add 19 parts of 200 mesh magnesia fine powder, 4 parts of silicon powder, 2 parts of α-alumina powder with a particle size of 3μm, and 0.15 parts of sodium hexametaphosphate and continue mixing for 5 minutes to obtain a regenerated tundish prefabricated castable;
[0073] The recycled tundish prefabricated castable is placed in a mixer, water is added and stirred for 5 minutes, and then slowly placed in a mold. Meanwhile, the vibration motor is turned on for 3 minutes. The mold and the embryo are placed in a curing kiln for curing for 24 hours (temperature 70°C, humidity 60%). The semi-finished product after demoulding is dried at 350°C*70h to obtain a finished tundish retaining wall.
[0074] In Example 6, the magnesium oxide content in the magnesia is >95%; the particle size of the silicon micropowder is 5-10 μm, and the silicon dioxide content in the silicon micropowder is >92%; the particle size of the α-alumina micropowder is 1-3 μm, and the aluminum oxide content is >99.5%; the additives are stainless steel fiber, organic fiber, and sodium hexametaphosphate.
[0075] The main physical and chemical indicators of sample 6 obtained in Example 6 are as follows: Mg ≥ 70%, Al2O3 ≥ 10%; the bulk density after baking at 110°C is ≥ 2.65 g / cm 3 The apparent porosity is ≤16.0%, the compressive strength (110℃×24h) is 40.8MPa, and the high temperature flexural strength (1400×0.3h) is 1.32MPa; Sample 6 was used on a double-flow slab middle package of a steel plant for 16 hours. After it was offline, the slag line of the retaining wall was corroded by 15mm, meeting the use requirements of the steel plant. Example
[0076] The preparation process of the tundish retaining wall is briefly described as follows:
[0077] Clean the steel slag and scrap steel on the surface of the used aluminum-magnesium carbon bricks to obtain the required aluminum-magnesium carbon brick waste blocks, and then crush the aluminum-magnesium carbon brick blocks to the required particle size, and remove iron while crushing to obtain recycled aluminum-magnesium carbon brick waste; the recycled aluminum-magnesium carbon brick waste includes: 13 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 8-15mm, 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 5-8mm, 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 3-5mm, and 15 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 1-3mm; the magnesium oxide content in the recycled aluminum-magnesium carbon brick waste is greater than 70%;
[0078] Select 16 parts of 0-1mm magnesia particles, 0.5 parts of organic fiber, and 1 part of steel fiber and mix them for 2 minutes, then add 19 parts of 200-mesh magnesia fine powder, 4.5 parts of silicon powder, 1.5 parts of α-alumina powder with a particle size of 3 μm, and 0.2 parts of sodium hexametaphosphate and continue mixing for 5 minutes to obtain a regenerated tundish prefabricated castable;
[0079] The recycled tundish prefabricated castable is placed in a mixer, water is added and stirred for 5 minutes, and then slowly placed in a mold. Meanwhile, the vibration motor is turned on for 3 minutes. The mold and the embryo are placed in a curing kiln for curing for 24 hours (temperature 70°C, humidity 60%). The semi-finished product after demoulding is dried at 350°C*70h to obtain a finished tundish retaining wall.
[0080] In Example 7, the magnesium oxide content in the magnesia is >95%; the particle size of the silicon micropowder is 5-10 μm, and the silicon dioxide content in the silicon micropowder is >92%; the particle size of the α-alumina micropowder is 1-3 μm, and the aluminum oxide content is >99.5%; the additives are stainless steel fiber, organic fiber, and sodium hexametaphosphate.
[0081] In the sample 7 obtained in Example 7, the main physical and chemical indicators are as follows: Mg ≥ 70%, Al2O3 ≥ 10%; the bulk density after baking at 110°C is ≥ 2.65 g / cm 3 The apparent porosity is ≤16.0%, the compressive strength (110℃×24h) is 41.7MPa, and the high temperature flexural strength (1400×0.3h) is 1.35MPa; Sample 7 was used on a double-flow slab middle package of a steel plant for 16 hours. After it was offline, the slag line of the retaining wall was corroded by 15mm, meeting the use requirements of the steel plant.
[0082] The recycled material tundish retaining walls obtained in Examples 1-7 can all meet the use requirements, successfully applying recycled aluminum-magnesium-carbon bricks in large quantities to tundish prefabricated products, and significantly reducing the cost of the tundish retaining walls.
[0083] Parts of the present invention not described in detail are prior art.
Claims
1. A method for preparing a tundish retaining wall using recycled materials, characterized in that: The following steps are involved: Step S1, preparing raw materials; the raw materials are calculated by mass, including 75-85 parts of recycled aluminum-magnesium carbon brick waste, 15-30 parts of magnesia sand, 2-5 parts of 92 silicon powder, 1-3 parts of α-alumina powder, and 0.2-4 parts of additives; the magnesium oxide content in the recycled aluminum-magnesium carbon brick waste is greater than 70%; the recycled aluminum-magnesium carbon brick waste is composed of the following components: 10-30 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 8-15mm, 10-25 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 5-8mm, 10-20 parts of recycled aluminum-magnesium carbon brick waste with a particle size of 3-5mm, and 1-3mm 10-20 parts of recycled aluminum-magnesium-carbon brick waste; the recycled aluminum-magnesium-carbon brick waste is obtained according to the following method: the steel slag and scrap steel on the surface of the used aluminum-magnesium-carbon waste brick are cleaned to obtain the required aluminum-magnesium-carbon brick waste bulk, and then the aluminum-magnesium-carbon brick bulk is crushed to the required particle size, and the iron removal treatment is performed while crushing, so as to finally obtain the recycled aluminum-magnesium-carbon brick waste; Step S2, mixing the recycled aluminum-magnesia-carbon brick waste, magnesia sand, silicon powder, α-alumina powder and additives to obtain a recycled tundish prefabricated castable; Step S3, forming, curing and drying the regenerated tundish prefabricated castable obtained in step S2 to obtain a tundish prefabricated product; the specific steps are as follows: S3.
1. Molding: put the prefabricated castable of the recycled tundish into a mixer, add water and stir for 5 minutes, slowly put it into the mold, and turn on the vibration motor for 3 minutes to shape the green body in the mold; Step S3.2, curing, placing the green body and the mold together in a curing kiln, curing for 24 hours, the curing temperature is 70°C, the humidity is 60%, and then demoulding to obtain a semi-finished product; the curing kiln is provided with a spray device, the spray device is used to control the humidity and dilute the ammonia released during the curing process of the green body; Step S3.3, drying: drying the semi-finished product at a temperature of 350°C for 70 hours to obtain a tundish retaining wall product.
2. The method for preparing a tundish retaining wall using recycled materials according to claim 1, characterized in that: In the step S1, the magnesia is composed of 0-1 mm magnesia particles and 200 mesh magnesia fine powder according to the following mass ratio: 10-18 parts of 0-1 mm magnesia particles and 15-20 parts of 200 mesh magnesia fine powder; the magnesium oxide content in the magnesia is greater than 95%.
3. The method for preparing a tundish retaining wall using recycled materials according to claim 1, characterized in that: In the step S1, the particle size of the 92 silicon micropowder is 5-10 μm, and the silicon dioxide content in the 92 silicon micropowder is greater than 92%.
4. The method for preparing a tundish retaining wall using recycled materials according to claim 1, characterized in that: In the step S1, the particle size of the α-alumina powder is 1-3 μm, and the alumina content is >99.5%.
5. The method for preparing a tundish retaining wall using recycled materials according to claim 1, characterized in that: In the step S2, the additive is stainless steel fiber, organic fiber, sodium hexametaphosphate or sodium tripolyphosphate.