Insulating material for drag chain cable and preparation method of insulating core for drag chain cable

By using insulating materials combined with SEBS and other materials in drag chain cables, and through electronic irradiation technology, the problem of easy damage of the insulating skin is solved, the tear resistance and mechanical properties of the insulating wire core are improved, and it is suitable for high-frequency bending. and low temperature environments, extend service life and improve UV resistance.

CN116515229BActive Publication Date: 2024-11-26JIANGSUSNGSHANG CABLE GROUP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310271625.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-11-26
Estimated Expiration
2043-03-20

AI Technical Summary

Technical Problem

The insulation of existing drag chain cables is prone to damage, resulting in reduced shielding performance and short service life, making it difficult to meet the high requirements of frequent bending and moving in industrial automation equipment.

Method used

Using SEBS as the main raw material, combining propylene elastomer, polyurethane, compatibility agent, antioxidant and ultraviolet light stabilizer, the tear resistance and mechanical properties of the insulated wire core are improved through electronic radiation technology, and through a specific extrusion process and the distribution ratio optimizes the processing performance of the material.

Benefits of technology

It significantly improves the tear resistance, mechanical properties and aging resistance of the insulated wire core, extends the service life, is suitable for high-frequency bending and low-temperature environments, and has excellent softness and ultraviolet resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004134890840000041
    Figure BDA0004134890840000041
  • Figure BDA0004134890840000051
    Figure BDA0004134890840000051
  • Figure BDA0004134890840000101
    Figure BDA0004134890840000101
Patent Text Reader

Abstract

The present application relates to the technical field of insulating materials, and specifically discloses a method for preparing an insulating material for a drag chain cable and an insulating wire core for a drag chain cable. The insulating material includes the following components: SEBS, propylene elastomer, polyurethane, white oil, compatibilizer, lubricant, masterbatch, antioxidant, ultraviolet light stabilizer, and crosslinking agent. The preparation method is as follows: SEBS and white oil are weighed in proportion and stirred; the remaining materials are weighed in proportion, stirred twice with the aforementioned materials, and then mixed and extruded to obtain insulating particles; the insulating particles are extruded on the outside of the conductor through an extrusion device to form an insulating skin layer, and then electron irradiated to obtain an insulating wire core, and the irradiation dose is 70~145Kgy. The present application electron irradiates the insulating skin layer, and the obtained insulating wire core has outstanding tear resistance, high-strength mechanical properties, and excellent softness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of cable insulation materials, and more specifically, to a method for preparing an insulating material for a drag chain cable and an insulating core for a drag chain cable. Background Art

[0002] In situations where equipment units need to move back and forth, in order to prevent the cables from getting tangled, worn, pulled off, and scattered, the cables are often placed in cable drag chains to protect them, and the cables can also move back and forth with the drag chains. In order to be more professionally used in various industrial automation equipment or in situations where there is frequent bending and movement, the drag chain cable needs to have excellent flexibility, wear resistance, and cyclic bending performance. To integrate the transmission of power and control signals, the drag chain cable needs to have better electrical performance, which places higher requirements on the insulation and sheath of the cable.

[0003] However, the current drag chain cable generally adopts soft PVC insulation and soft PVC sheath insulation. Its disadvantage is that when working for a long time, the core wire is squeezed and deformed, the insulation skin is damaged, and the braided shielding net is damaged, which affects the shielding performance, shortens the service life, and seriously affects the electrical performance. Summary of the invention

[0004] In order to improve the defect that the insulation skin of a drag chain cable is easily damaged after long-term use, the present application provides an insulating material for a drag chain cable and a method for preparing an insulating core for a drag chain cable.

[0005] In the first aspect, the present application provides an insulating material for a drag chain cable, comprising the following components in parts by weight: 40 to 60 parts of SEBS, 10 to 20 parts of propylene elastomer, 10 to 20 parts of polyurethane, 10 to 20 parts of white oil, 5 to 10 parts of compatibilizer, 2 to 4 parts of lubricant, 1 part of masterbatch, 0.4 to 0.8 parts of antioxidant, 0.3 to 0.6 parts of UV stabilizer, and 1 to 2 parts of cross-linking agent.

[0006] This application uses SEBS as the main raw material for drag chain cable insulation. SEBS material has good temperature resistance, its brittle temperature is ≤-60°C, and the maximum operating temperature reaches 149°C; it also has excellent electrical properties and aging resistance. In addition, since the SEBS resin itself has a loose and porous structure, the processing performance of the SEBS material can be improved by absorbing white oil.

[0007] Preferably, the SEBS is a linear structured SEBS, with a styrene content of 29 wt% to 33 wt% and a toluene solution viscosity of 500 to 2000 mPa.s at 25°C.

[0008] The present application uses a linear structured SEBS, which has better rheological properties for extrusion processing and can ensure the processability of the main pellets. The linear structured SEBS has the characteristics of large molecular weight and long molecular chain, which can further provide more physical crosslinking points to obtain higher strength. At the same time, the linear structured SEBS has good oil absorption and oil locking properties.

[0009] Preferably, the density of the propylene elastomer is 0.860-0.875 g / cm 3 Its melt index at 190°C and 2.16kg is 1-5g / 10min.

[0010] Propylene elastomer has good compatibility with SEBS. The present application can improve the mechanical properties of the material by introducing propylene elastomer, and can effectively solve the problem of uneven extruded surface of low-oil-filled SEBS material.

[0011] Preferably, the polyurethane is aliphatic polyurethane with a hardness of 80-90A.

[0012] Polyurethane has excellent tear resistance and repeated bending and twisting performance. Polyurethane can be divided into aliphatic and aromatic types according to the type of isocyanate used. This application prefers aliphatic polyurethane, which has better tear strength and mechanical properties than aromatic polyurethane. Moreover, aliphatic polyurethane has better light resistance stability.

[0013] Preferably, the compatibilizer is maleic anhydride grafted SEBS polymer.

[0014] In order to further improve the compatibility between different resins, the present application adds a compatibilizer to enhance the interaction between material molecules, thereby enhancing mechanical properties and tear resistance. The present application uses maleic anhydride grafted SEBS polymer as a compatibilizer, which allows the components in the system to form a composite matrix component to ensure good bonding performance, high resilience and heat resistance.

[0015] Preferably, the antioxidant consists of a primary antioxidant and an auxiliary antioxidant, wherein the primary antioxidant is antioxidant 1098, antioxidant 1790 or antioxidant 245, and the auxiliary antioxidant is antioxidant 126 or antioxidant 264.

[0016] By adding antioxidants, the depolymerization reaction rate of polymers can be significantly slowed down under aging conditions, and the molecular fragmentation or carbonaceous residue generation can be significantly reduced. Since the degradation process starts at the molecular chain end or other weak links in the molecule, the connected monomer chain links are lost one by one. The antioxidant formed by compounding the main antioxidant with the auxiliary antioxidant in this application can isolate free radicals as intermediates and react with the polymer to generate new free radicals, thereby controlling the degradation rate and greatly improving the long-term aging resistance of the insulating cortex.

[0017] Preferably, the ultraviolet light stabilizer includes at least one of UV-944 and UV-770, and at least one of UV-234, UV-328 and UV-622.

[0018] By adopting the above technical solution, ultraviolet rays can be absorbed after cabling, so that the insulation material can be extruded with a smooth surface and fast speed, with less smoke during extrusion, and will not turn yellow under light after cabling. By compounding the above main and auxiliary antioxidants with different types of ultraviolet light stabilizers, the material's anti-ultraviolet performance and weather resistance can be significantly improved.

[0019] Preferably, the crosslinking agent includes at least one of trimethylolpropane trimethacrylate and triallyl isocyanurate.

[0020] By adopting the above technical solution, the proportion of the cross-linking reaction can be increased and the speed of the cross-linking reaction can be improved.

[0021] In a second aspect, the present application provides a method for preparing an insulated wire core for a drag chain cable, comprising the following steps:

[0022] Step S1: weigh SEBS and white oil in proportion and add them into a high-speed mixer for stirring;

[0023] Step S2: weigh the remaining materials in proportion, and put them into a high-speed mixer together with the materials obtained in step S1 for secondary stirring. After the secondary stirring, transfer the materials to a twin-screw loss-in-weight scale to start mixing, extrusion and granulation to obtain insulating particles;

[0024] Step S3: Extruding the insulating particles obtained in step S2 onto the outside of the conductor through an extrusion device to form an insulating layer, and then subjecting the conductor to electron irradiation to obtain an insulated wire core, wherein the electron beam energy used for irradiation is 2.7 MeV, the electron beam current intensity is 18-32 mA, and the irradiation dose is 70-145 Kgy.

[0025] By adopting the above technical solution, the cross-linking degree of the material after irradiation can be guaranteed, and the thermal extension can be controlled within an appropriate range, ensuring that the material has both good tensile strength and excellent tear resistance. In this application, the insulating core obtained by electron irradiating the insulating skin layer has outstanding tear resistance, high-strength mechanical properties, and excellent softness.

[0026] Preferably, the insulating particles are extruded through a twin-screw extruder, and the temperature of each zone is set as follows: barrel zone 1: 145±5°C, barrel zone 2: 155±5°C, barrel zone 3: 165±5°C, barrel zone 4: 170±5°C, barrel zone 5: 175±5°C, barrel zone 6: 180±5°C, barrel zone 7: 180±5°C, barrel zone 8: 190±5°C, barrel zone 9: 195±5°C, and die head: 195±5°C;

[0027] Alternatively, the insulating particles are extruded through a single-screw extruder, and the temperature of each zone is set as: body zone 1: 155±5°C, body zone 2: 160±5°C, body zone 3: 170±5°C, body zone 4: 180±5°C, body zone 5: 185±5°C, head zone 1: 185±5°C, head zone 2: 185±5°C, head zone 3: 185±5°C, extrusion pressure 20~30MPa; screw speed 15~30rpm, traction speed 20~40m / min.

[0028] The present application provides two processes for the extrusion equipment of insulating particles, namely a single-screw extruder and a twin-screw extruder, which have wider adaptability.

[0029] In summary, this application has the following beneficial effects:

[0030] 1. This application uses SEBS as the main raw material for drag chain cable insulation. SEBS material has good temperature resistance, its brittle temperature is ≤-60°C, and the maximum operating temperature reaches 149°C; it also has excellent electrical properties and aging resistance. In addition, since the SEBS resin itself has a loose and porous structure, the processing performance of the SEBS material can be improved by absorbing white oil.

[0031] 2. The present application performs electron irradiation on the extruded insulation layer, and the obtained insulation core has outstanding tear resistance, high-strength mechanical properties, and excellent softness. DETAILED DESCRIPTION

[0032] The present application is further described in detail below with reference to the embodiments.

[0033] The raw materials involved in the following preparation examples and embodiments of the present application include:

[0034] SEBS, G1651 from Kraton, USA; Propylene elastomer, ExxonMobil 3000; Polyurethane, BASF 685A; White oil, Changzhou Kairun 36# white oil; Compatibilizer, Taiwan Rubber 7126; Lubricant, Hanwei zinc stearate; Masterbatch, Shanghai Wujiang 40-or-1964; Antioxidant 1098, BASF (China) Co., Ltd., CAS registration number is 245-442-7; Antioxidant 1790, American Artifact Antioxidant Company, CAS registration number is 40601-76-1; Antioxidant 245, Beijing Jiyi Chemical Co., Ltd., CAS registration number is 36443-68-2; Antioxidant 126, BASF (China) Co., Ltd., CAS registration number is 26741-53-7; Antioxidant 264, Lianyungang Ningkang Chemical Co., Ltd., CAS registration number is UV-944, Jiangsu Suqian Liansheng Chemical Co., Ltd., CAS registration number is 70624-18-9; UV-770, BASF (China) Co., Ltd., CAS registration number is 52829-07-9; UV-234, Beijing Tiangang Additive Co., Ltd., CAS registration number is 70321-86-7; UV-328, Beijing Tiangang Additive Co., Ltd., CAS registration number is 25973-55-1; UV-622, Jiangsu Suqian Liansheng Chemical Co., Ltd., CAS registration number is 65447-77-0; crosslinker TAIC, Hangzhou Keli Chemical, CAS registration number is 1025-15-6; crosslinker TMPTMA, Sigma-Aldrich, CAS registration number is 3290-92-4.

[0035] The device used for the electron irradiation process in the present application is a DD3.0-30 / 1200 high frequency and high voltage electron accelerator. The conductors used in the following embodiments of the present application are all copper conductors.

[0036] Preparation Example 1-10

[0037] Preparation Examples 1-10 respectively provide an insulating particle for a drag chain cable, and the formula of each component thereof is shown in Table 1 (all are weight fractions). Among them, Preparation Examples 1-9 are prepared using the same preparation method and equipment, specifically including:

[0038] Step S1: Weigh SEBS and white oil in proportion and add them into a high-speed mixer, stirring for 5 minutes;

[0039] Step S2: weigh the remaining materials in proportion, and put them into a high-speed mixer together with the materials obtained in step S1 for secondary stirring for 15 minutes. After the secondary stirring, transfer the materials to a twin-screw extruder and start mixing, extrusion and granulation to obtain insulating particles of 4mm×4mm×3mm, wherein the temperature of each zone of the twin-screw extruder is set to: barrel zone 1: 145±5°C, barrel zone 2: 155±5°C, barrel zone 3: 165±5°C, barrel zone 4: 170±5°C, barrel zone 5: 175±5°C, barrel zone 6: 180±5°C, barrel zone 7: 180±5°C, barrel zone 8: 190±5°C, barrel zone 9: 195±5°C, and head: 195±5°C.

[0040] Preparation Example 10 was prepared using the following preparation method and equipment, specifically including:

[0041] Step S1: Weigh SEBS and white oil in proportion and add them into a high-speed mixer, stirring for 5 minutes;

[0042] Step S2: weigh the remaining materials in proportion, and put them into a high-speed mixer together with the materials obtained in step S1 for secondary stirring for 15 minutes. After the secondary stirring, transfer the materials to a single-screw extruder and start mixing, extrusion and granulation to obtain insulating particles, wherein the temperature of each zone of the single-screw extruder is set to: body zone 1: 155±5°C, body zone 2: 160±5°C, body zone 3: 170±5°C, body zone 4: 180±5°C, body zone 5: 185±5°C, head zone 1: 185±5°C, head zone 2: 185±5°C, head zone 3: 185±5°C, extrusion pressure 20MPa; screw speed 15rpm, traction speed 20m / min.

[0043] Table 1

[0044]

[0045]

[0046] Example 1

[0047] The insulating particles obtained in Preparation Example 1 were extruded at 14 mm 2 The conductor is extruded to form an insulating layer with an average thickness of 1 mm, and then the insulating layer is electron irradiated to obtain an insulated wire core. The specific irradiation process is as follows: the electron beam energy is 2.7 MeV, the number of turns is 14, the electron beam current intensity is 20 mA, the line speed is 50 m / min, and the irradiation dose is 70 Kgy. After irradiation, it is parked for at least 24 hours.

[0048] Example 2

[0049] The insulating particles obtained in Preparation Example 1 were extruded at 95 mm2 The conductor is extruded to form an insulating layer with an average thickness of 1.6 mm, and then the insulating layer is electron irradiated to obtain an insulated wire core. The specific irradiation process is as follows: the electron beam energy is 2.7 MeV, the number of turns is 14, the electron beam current intensity is 24 mA, the line speed is 60 m / min, and the irradiation dose is 95 Kgy. After irradiation, it is parked for at least 24 hours.

[0050] Example 3

[0051] The insulating particles obtained in Preparation Example 1 were extruded at 150 mm 2 The conductor is extruded to form an insulating layer with an average thickness of 1.8 mm, and then the insulating layer is electron irradiated to obtain an insulated wire core. The specific irradiation process is as follows: the electron beam energy is 2.7 MeV, the number of turns is 7, the electron beam current intensity is 28 mA, the line speed is 20 m / min, and the irradiation dose is 120 Kgy. After irradiation, it is parked for at least 24 hours.

[0052] Example 4

[0053] The insulating particles obtained in Preparation Example 1 were extruded at 185 mm 2 The conductor is extruded to form an insulating layer with an average thickness of 2.0 mm, and then the insulating layer is electron irradiated to obtain an insulated wire core. The specific irradiation process is as follows: the electron beam energy is 2.7 MeV, the number of turns is 7, the electron beam current intensity is 28 mA, the line speed is 18 m / min, and the irradiation dose is 135 Kgy. After irradiation, it is parked for at least 24 hours.

[0054] Example 5

[0055] The insulating particles obtained in Preparation Example 1 were extruded at 240 mm 2 The conductor is extruded to form an insulating layer with an average thickness of 2.2 mm, and then the insulating layer is electron irradiated to obtain an insulated wire core. The specific irradiation process is as follows: the electron beam energy is 2.7 MeV, the number of turns is 7, the electron beam current intensity is 32 mA, the line speed is 17 m / min, and the irradiation dose is 145 Kgy. After irradiation, it is parked for at least 24 hours.

[0056] Example 6

[0057] The insulating particles obtained in Preparation Example 2 were extruded at 240 mm 2 The conductor is extruded to form an insulating layer with an average thickness of 2.2 mm, and then the insulating layer is electron irradiated to obtain an insulated wire core. The specific irradiation process is as follows: the electron beam energy is 2.7 MeV, the number of turns is 7, the electron beam current intensity is 32 mA, the line speed is 17 m / min, and the irradiation dose is 145 Kgy. After irradiation, it is parked for at least 24 hours.

[0058] Example 7

[0059] The insulating particles obtained in Preparation Example 3 were extruded at 240 mm 2 The conductor is extruded to form an insulating layer with an average thickness of 2.2 mm, and then the insulating layer is electron irradiated to obtain an insulated wire core. The specific irradiation process is as follows: the electron beam energy is 2.7 MeV, the number of turns is 7, the electron beam current intensity is 32 mA, the line speed is 17 m / min, and the irradiation dose is 145 Kgy. After irradiation, it is parked for at least 24 hours.

[0060] Example 8

[0061] The insulating particles obtained in Preparation Example 4 were extruded at 240 mm 2 The conductor is extruded to form an insulating layer with an average thickness of 2.2 mm, and then the insulating layer is electron irradiated to obtain an insulated wire core. The specific irradiation process is as follows: the electron beam energy is 2.7 MeV, the number of turns is 7, the electron beam current intensity is 32 mA, the line speed is 17 m / min, and the irradiation dose is 145 Kgy. After irradiation, it is parked for at least 24 hours.

[0062] Example 9

[0063] The insulating particles obtained in Preparation Example 5 were extruded at 240 mm 2 The conductor is extruded to form an insulating layer with an average thickness of 2.2 mm, and then the insulating layer is electron irradiated to obtain an insulated wire core. The specific irradiation process is as follows: the electron beam energy is 2.7 MeV, the number of turns is 7, the electron beam current intensity is 32 mA, the line speed is 17 m / min, and the irradiation dose is 145 Kgy. After irradiation, it is parked for at least 24 hours.

[0064] Example 10

[0065] The insulating particles obtained in Preparation Example 6 were extruded at 240 mm 2 The conductor is extruded to form an insulating layer with an average thickness of 2.2 mm, and then the insulating layer is electron irradiated to obtain an insulated wire core. The specific irradiation process is as follows: the electron beam energy is 2.7 MeV, the number of turns is 7, the electron beam current intensity is 32 mA, the line speed is 17 m / min, and the irradiation dose is 145 Kgy. After irradiation, it is parked for at least 24 hours.

[0066] Embodiment 11

[0067] The insulating particles obtained in Preparation Example 7 were extruded at 240 mm 2The conductor is extruded to form an insulating layer with an average thickness of 2.2 mm, and then the insulating layer is electron irradiated to obtain an insulated wire core. The specific irradiation process is as follows: the electron beam energy is 2.7 MeV, the number of turns is 7, the electron beam current intensity is 32 mA, the line speed is 17 m / min, and the irradiation dose is 145 Kgy. After irradiation, it is parked for at least 24 hours.

[0068] Example 12

[0069] The insulating particles obtained in Preparation Example 8 were extruded at 240 mm 2 The conductor is extruded to form an insulating layer with an average thickness of 2.2 mm, and then the insulating layer is electron irradiated to obtain an insulated wire core. The specific irradiation process is as follows: the electron beam energy is 2.7 MeV, the number of turns is 7, the electron beam current intensity is 32 mA, the line speed is 17 m / min, and the irradiation dose is 145 Kgy. After irradiation, it is parked for at least 24 hours.

[0070] Example 13

[0071] The insulating particles obtained in Preparation Example 9 were extruded at 240 mm 2 The conductor is extruded to form an insulating layer with an average thickness of 2.2 mm, and then the insulating layer is electron irradiated to obtain an insulated wire core. The specific irradiation process is as follows: the electron beam energy is 2.7 MeV, the number of turns is 7, the electron beam current intensity is 32 mA, the line speed is 17 m / min, and the irradiation dose is 145 Kgy. After irradiation, it is parked for at least 24 hours.

[0072] Embodiment 14

[0073] The insulating particles obtained in Preparation Example 10 were extruded at 240 mm 2 The conductor is extruded to form an insulating layer with an average thickness of 2.2 mm, and then the insulating layer is electron irradiated to obtain an insulated wire core. The specific irradiation process is as follows: the electron beam energy is 2.7 MeV, the number of turns is 7, the electron beam current intensity is 32 mA, the line speed is 17 m / min, and the irradiation dose is 145 Kgy. After irradiation, it is parked for at least 24 hours.

[0074] Comparative Example 1

[0075] The insulating particles obtained in Preparation Example 1 were extruded at 240 mm 2 The conductor is extruded to form an insulating layer with an average thickness of 2.2 mm, and then the insulating layer is electron irradiated to obtain an insulated wire core. The specific irradiation process is as follows: the electron beam energy is 2.7 MeV, the number of turns is 7, the electron beam current intensity is 32 mA, the line speed is 17 m / min, and the irradiation dose is 120 Kgy. After irradiation, it is parked for at least 24 hours.

[0076] Comparative Example 2

[0077] The insulating particles obtained in Preparation Example 1 were extruded at 240 mm 2 The conductor is extruded to form an insulating layer with an average thickness of 2.2 mm, and then the insulating layer is electron irradiated to obtain an insulated wire core. The specific irradiation process is as follows: the electron beam energy is 2.7 MeV, the number of turns is 7, the electron beam current intensity is 32 mA, the line speed is 17 m / min, and the irradiation dose is 100 Kgy. After irradiation, it is parked for at least 24 hours.

[0078] Comparative Example 3

[0079] The insulating particles obtained in Preparation Example 1 were extruded at 240 mm 2 The conductor is extruded to form an insulating layer with an average thickness of 2.2 mm, and then the insulating layer is electron irradiated to obtain an insulated wire core. The specific irradiation process is as follows: the electron beam energy is 2.7 MeV, the number of turns is 7, the electron beam current intensity is 32 mA, the line speed is 17 m / min, and the irradiation dose is 70 Kgy. After irradiation, it is parked for at least 24 hours.

[0080] Comparative Example 4

[0081] Comparative Example 4 provides an insulating particle for a drag chain cable and an insulating core prepared using the insulating particle. The preparation method of the insulating particle of Comparative Example 4 is the same as that of Preparation Example 1, and the formula of each component is basically the same as that of Preparation Example 1, with the only difference being that the mass fraction of propylene elastomer is 8 parts.

[0082] The above insulating particles are extruded through a 240mm 2 The conductor is extruded to form an insulating layer with an average thickness of 2.2 mm, and then the insulating layer is electron irradiated to obtain an insulated wire core. The specific irradiation process is as follows: the electron beam energy is 2.7 MeV, the number of turns is 7, the electron beam current intensity is 32 mA, the line speed is 17 m / min, and the irradiation dose is 145 Kgy. After irradiation, it is parked for at least 24 hours.

[0083] Comparative Example 5

[0084] Comparative Example 5 provides an insulating particle for a drag chain cable and an insulating core prepared using the insulating particle. The preparation method of the insulating particle of Comparative Example 5 is the same as that of Preparation Example 1, and the formula of each component is basically the same as that of Preparation Example 1, with the only difference being that the mass fraction of propylene elastomer is 21 parts.

[0085] The above insulating particles are extruded through a 240mm 2The conductor is extruded to form an insulating layer with an average thickness of 2.2 mm, and then the insulating layer is electron irradiated to obtain an insulated wire core. The specific irradiation process is as follows: the electron beam energy is 2.7 MeV, the number of turns is 7, the electron beam current intensity is 32 mA, the line speed is 17 m / min, and the irradiation dose is 145 Kgy. After irradiation, it is parked for at least 24 hours.

[0086] Performance Testing

[0087] The insulated wire cores prepared in Examples 1-14 and Comparative Examples 1-5 were subjected to performance tests. The test results of tensile strength and elongation at break test, thermal extension test, thermal deformation test, and thermal shock test are shown in Table 2, and the test results of cold bending test, thermal aging test, and UV aging resistance test are shown in Table 3.

[0088] 1. Tensile strength and elongation at break test: The same length of the conductor-containing insulating layer prepared in Examples 1-14 and Comparative Examples 1-5 was cut as a test sample, and the tensile strength and elongation at break of the samples were tested with reference to GB / T 2951.11-2008 "General test methods for insulation and sheathing materials of electric and optical cables Part 11: General test methods - Thickness and dimensional measurement - Mechanical properties test".

[0089] 2. Thermal elongation test: The same length of the insulating layer containing the conductor prepared in Examples 1-14 and Comparative Examples 1-5 was cut as a test sample, and the thermal elongation of the samples under load and the permanent deformation rate after the samples were cooled were tested with reference to GB / T 2951.21-2008 "General test methods for insulation and sheath materials of electric and optical cables Part 21: Special test methods for elastomeric mixtures. Ozone resistance test-Hot elongation test-Mineral oil immersion test".

[0090] 3. Thermal deformation test: The same length of the insulating layer containing the conductor prepared in Examples 1-14 and Comparative Examples 1-5 was cut as a sample, and the samples were tested with reference to Section 7.7 of the UL2556 "Test Methods for Wires and Cables" standard on thermal deformation. The test conditions were a load of 250g, a load time of 1 hour, and a test temperature of 121°C. The deformation of the sample after the test was measured, and the heating deformation rate was calculated.

[0091] 4. Thermal shock test: The same length of the insulating layer containing the conductor prepared in Examples 1-14 and Comparative Examples 1-5 was cut as a sample, and the samples were tested with reference to Section 7.2 of the UL2556 "Test Methods for Wires and Cables" standard on thermal shock. The test conditions were: load time of 1 hour and test temperature of 121°C. Observe whether the sample surface has cracks.

[0092] 5. Cold bending test: The same length of the insulating layer containing the conductor prepared in Examples 1-14 and Comparative Examples 1-5 was cut as a sample, and the sample was subjected to a cold bending test according to the method in Section 5.3.3 of the cold bending test of UL62 "Safety Standard for Flexible Wires and Cables". The test conditions were: the test temperature was -30°C and the test time was 4 hours. Observe whether the sample surface was cracked.

[0093] 6. Heat aging test: The same length of the insulating layer containing the conductor prepared in Examples 1-14 and Comparative Examples 1-5 was cut as a sample, and the test was carried out with reference to GB / T 2951.12-2008 "General test methods for insulation and sheath materials of electric and optical cables Part 12: General test methods - Heat aging test method"; the heat aging conditions were: aging temperature of 136°C, aging time of 240h, then the appearance of the sample was observed for cracks, and tensile strength and elongation at break were tested, and the tensile strength retention rate and elongation at break retention rate of the sample were calculated.

[0094] 7. UV aging resistance test: The same length of the conductor-containing insulating layer prepared in Examples 1-14 and Comparative Examples 1-5 was cut as a sample, and irradiated with a 6kW xenon lamp and sprayed with water at a water pressure of 0.12-0.29MPa. The ultraviolet irradiation was performed in a cycle of 120 minutes, of which 18 minutes were for simultaneous water spraying and irradiation, and the other 102 minutes were for single irradiation, for a total of 1000 hours of exposure. The samples were then placed at room temperature for 20 hours, and the appearance of the samples was observed. There should be no cracks in the appearance. The tensile strength and elongation at break tests were performed, and the tensile strength retention rate and elongation at break retention rate of the samples were calculated.

[0095] Table 2

[0096]

[0097]

[0098] Table 3

[0099]

[0100] It can be seen from the test results of Examples 1 to 5 that the formula of the insulating particles provided in Preparation Example 1 of the present application can be applied to the extrusion of the insulating skin layer outside the conductors of different thicknesses. Since the thickness of the insulating skin layer required for conductors of different thicknesses is different, the present application determines the size of the irradiation dose according to the thickness of the insulating skin layer to ensure that the absorbed dose of the material is consistent. In addition, the present application can ensure that the material has high tear strength and tensile strength by limiting the irradiation dose and irradiation process parameters within a suitable range.

[0101] It can be seen from the test results of Example 1 and Examples 5-14 that the present application uses SEBS as the main raw material of the drag chain cable insulation material and combines it with the component formula provided in the present application to obtain an insulating layer with excellent mechanical properties, excellent anti-aging properties and excellent low-temperature resistance.

[0102] It can be seen from the test results of Example 5 and Comparative Examples 1-3 that the difference between them lies in the different irradiation doses, and the irradiation dose of Example 5 is greater than that of Comparative Examples 1-3. Although the tensile strength and elongation at break of the insulating skin obtained by Comparative Examples 1-3 are relatively high, after the thermal extension test, the permanent deformation rate reaches more than 5%, and the thermal deformation rate increases significantly. Even Comparative Examples 2 and 3 have thermal shock cracking. Comparative Example 3 also fails to pass the cold bending test, and the retention rates of tensile strength and elongation at break after the thermal aging test and the UV aging test are both low. This shows that the insulating particles obtained by using Preparation Example 1 are extruded at 240mm 2 When the conductor is extruded to form an insulating layer with an average thickness of 2.2 mm, at least 145 Kgy of radiation dose should be provided for radiation cross-linking so that the material can obtain good mechanical properties.

[0103] It can be seen from the test results of Example 5, Examples 13-14 and Comparative Examples 4-5 that the amount of propylene elastomer in the formula of the insulating particles used in Examples 5, 13 and 14 is 10-20 parts, while the amount of propylene elastomer in the formula of the insulating particles used in Comparative Examples 4 and 5 is 8 parts and 21 parts respectively. The results show that the mechanical properties of the insulating skin obtained in Comparative Examples 4 and 5 are both reduced, and Comparative Example 4 fails to pass the cold bending test. The retention rate of tensile strength and elongation at break of Comparative Example 5 after the heat aging test and the UV aging test is reduced. This shows that the use of 10-20 parts of propylene insulation can make the insulating skin obtain good low temperature resistance and aging resistance.

[0104] Usually, the degree of cross-linking of the wire core is generally replaced by the method of testing the thermal elongation. The thermal elongation decreases with the increase of the irradiation dose until it reaches saturation. Underdose or overdose will affect other performance indicators. After sampling and testing the data, it was found that the thermal elongation is close to saturation below 20%, and the original tensile strength and elongation at break have small margins; when it is above 40%, the tear resistance fluctuates greatly. After multiple rounds of testing, it was found that when the thermal elongation is within 20%-40%, the performance of the wire core after irradiation is relatively stable. Therefore, when the electron irradiation is performed in this application, the thermal elongation of the material is controlled at 20%-40%. During irradiation, the irradiation dose is determined according to the thickness of the insulating skin layer (see Examples 1-5 of this application) to ensure that the absorbed dose of the material is consistent.

[0105] In summary, the insulating cortex provided by the present application has the advantages of not cracking in a low temperature environment of -30°C and not cracking in a high temperature environment of 121°C. It is applicable to a wide range of ambient temperatures, and is especially suitable for long-term reciprocating bending and twisting conditions of drag chain cables, without cracking or deformation. In addition, since the cable connector may need to be exposed to the natural environment for a long time, the insulating cortex provided by the present application also has excellent resistance to heat aging and UV aging, which can just meet the aforementioned operating conditions. At the same time, the insulating cortex provided by the present application also has excellent softness, high-strength mechanical properties and outstanding tear resistance, which meet the use requirements of drag chain cables to a great extent.

[0106] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An insulating material for a drag chain cable, It is characterized in that The composition comprises the following components in parts by weight: 40-60 parts of SEBS, 10-20 parts of propylene elastomer, 10-20 parts of polyurethane, 10-20 parts of white oil, 5-10 parts of compatibilizer, 2-4 parts of lubricant, 1 part of masterbatch, 0.4-0.8 parts of antioxidant, 0.3-0.6 parts of ultraviolet light stabilizer, and 1-2 parts of crosslinking agent; the SEBS is a linear structure SEBS, the styrene content is 29wt%-33wt%, and the toluene solution viscosity at 25°C is 500-2000mPa.s.

2. The insulating material for drag chain cables according to claim 1, It is characterized in that The density of the propylene elastomer is 0.860-0.875 g / cm 3 Its melt index at 190°C and 2.16kg is 1~5g / 10min.

3. The insulating material for drag chain cables according to claim 1, It is characterized in that The polyurethane is aliphatic polyurethane with a hardness of 80-90A.

4. The insulating material for drag chain cables according to claim 1, It is characterized in that The compatibilizer is maleic anhydride grafted SEBS polymer.

5. The insulating material for drag chain cables according to claim 1, It is characterized in that The antioxidant consists of a main antioxidant and an auxiliary antioxidant, wherein the main antioxidant is antioxidant 1098, antioxidant 1790 or antioxidant 245, and the auxiliary antioxidant is antioxidant 126 or antioxidant 264.

6. The insulating material for drag chain cables according to claim 1, It is characterized in that The ultraviolet light stabilizer includes at least one of UV-944 and UV-770, and at least one of UV-234, UV-328 and UV-622.

7. The insulating material for drag chain cables according to claim 1, It is characterized in that The crosslinking agent includes at least one of trimethylolpropane trimethacrylate and triallyl isocyanurate.

8. A method for preparing an insulated wire core for a drag chain cable according to any one of claims 1 to 7, It is characterized in that The steps include: Step S1: weigh SEBS and white oil in proportion and add them into a high-speed mixer for stirring; Step S2: weigh the remaining materials in proportion, and put them into a high-speed mixer together with the materials obtained in step S1 for secondary stirring. After the secondary stirring, transfer the materials to a screw extruder to start mixing, extruding and granulating to obtain insulating particles; Step S3: Extruding the insulating particles obtained in step S2 onto the outside of the conductor through an extrusion device to form an insulating layer, and then subjecting the conductor to electron irradiation to obtain an insulated wire core, wherein the electron beam energy used for irradiation is 2.7 Mev, the electron beam current intensity is 18-32 mA, and the irradiation dose is 70-145 Kgy.

9. The method for preparing the insulated wire core for the drag chain cable according to claim 8, It is characterized in that The insulating particles are extruded through a twin-screw extruder, and the temperature of each zone is set as follows: barrel zone 1: 145±5°C, barrel zone 2: 155±5°C, barrel zone 3: 165±5°C, barrel zone 4: 170±5°C, barrel zone 5: 175±5°C, barrel zone 6: 180±5°C, barrel zone 7: 180±5°C, barrel zone 8: 190±5°C, barrel zone 9: 195±5°C, and die head: 195±5°C; Alternatively, the insulating particles are extruded through a single-screw extruder, and the temperature of each zone is set as: body zone 1: 155±5℃, body zone 2: 160±5℃, body zone 3: 170±5℃, body zone 4: 180±5℃, body zone 5: 185±5℃, head zone 1: 185±5℃, head zone 2: 185±5℃, head zone 3: 185±5℃, extrusion pressure 20~30MPa; screw speed 15~30rpm, traction speed 20~40m / min.

Citation Information

Patent Citations

  • Delay drainage valve for cistern of toilet closet

    CN2454427Y

  • Oil-resistant halogen-free flame retardant TPE (Thermo Plastics Elastomer) cable material and preparation method thereof

    CN106398083A

  • TPE sheath material for irradiation crosslinking 125 DEG C charging pile and preparation method of TPE sheath material

    CN107011574A

  • Halogen-free thermoplastic elastomer insulating material and preparation method thereof

    CN110527236A

  • Wear-resistant and high-resilience-rate TPE caster material used for bonding pp, and preparation method

    WO2017084216A1