Compositions, methods of their manufacture, and articles thereof
By using compositions of polyetherimide, poly(aryl ether sulfone), or cyclic olefin copolymers with specific fillers, the problem of deformation and discoloration of thermoplastic polymers at high temperatures has been solved, resulting in optical materials with low coefficients of thermal expansion and high infrared transmittance.
Patent Information
- Application Number
- CN202180081198.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-12-02
- Filing Date
- 2021-11-23
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2041-11-23
AI Technical Summary
Existing thermoplastic polymer materials cannot maintain dimensional stability and good optical properties at high temperatures, making it difficult to meet the needs of optical applications. In particular, they are prone to deformation or discoloration when used under high-temperature conditions.
Compositions containing polyetherimide, poly(aryl ether sulfone), or cyclic olefin copolymers and specific fillers are blended and heat-treated to form compositions with low coefficients of thermal expansion suitable for optical applications.
A composition with a low coefficient of thermal expansion and high infrared transmittance is provided, suitable for optical applications, maintaining good optical properties and being stable at high temperatures.
Smart Images

Figure BDA0004262153880000031 
Figure BDA0004262153880000032 
Figure BDA0004262153880000041
Abstract
Description
[0001] Citations of relevant applications
[0002] This application claims priority and benefit to European Patent Application No. 20211292.6, filed on 2 December 2020, the entire contents of which are incorporated herein by reference. Background Technology
[0003] Thermoplastic polymers, including polyetherimides and polysulfones, are used to manufacture articles and assemblies for a wide range of applications, from automotive parts to electronic devices. Due to their beneficial properties such as transparency and impact resistance, polyetherimides and polysulfones have also been used in optical applications, including as sensor lenses, optical interconnects, transceivers, light guides, camera lenses, eyeglass and safety glass lenses, lighting lenses (such as lamps, flashlights, and lantern lenses), and headlight lenses and covers for motor vehicles. Because many optical products are used in high-temperature environments or must be processed under harsh conditions, it is desirable for materials to withstand high temperatures without deformation or discoloration, and to maintain good optical properties even when processed using conventional molding processes. To date, many optical lenses have been made of glass because polymer materials cannot provide the necessary dimensional stability, particularly for single-mode fiber optic connectors.
[0004] Therefore, there is a persistent need in the art for improved compositions particularly suitable for optical applications. Providing compositions with a low coefficient of thermal expansion and high infrared transmittance would be especially advantageous. Summary of the Invention
[0005] The composition comprises greater than 50 wt% to less than 75 wt% of polyetherimide, poly(aryl ether sulfone), or cyclic olefin copolymer; and greater than 25 wt% to less than 50 wt% of filler; wherein, when the polymer comprises polyetherimide, the filler comprises fibers having an average fiber diameter of 5 micrometers to 10 micrometers and an average fiber length of 55 micrometers to 75 micrometers, and a fiber diameter of 2.5 m. 2 / g to less than 2.9m 2 Wollastonite fibers with a surface area of / g, a bulk density of 0.42g / cc to 0.50g / cc, and a silica content of 52% to 55%; or boehmite having an average particle size (D50) of 0.4 μm to less than 0.9 μm as determined by laser scattering; when the polymer includes poly(arylene ether sulfone), the filler comprises fibers with an average fiber diameter of 1 μm to 5 μm and an average fiber length of 5 μm to 12 μm, and a surface area of / g. 2 / g to 4.3m 2Wollastonite fibers with a surface area of / g and a bulk density of 0.48g / cc to 0.56g / cc; or boehmite having an average particle size (D50) of 0.4 μm to less than 0.9 μm as determined by laser scattering; and when the polymer includes a cyclic olefin copolymer, the filler includes fibers with an average fiber diameter of 10 μm to 15 μm and an average fiber length of 140 μm to 165 μm, 1.0m 2 / g to 1.8m 2 / g surface area and 0.18g / cc to 0.26g / cc bulk density of wollastonite fibers; wherein, weight percentage is based on the total weight of the composition.
[0006] The method for preparing the composition includes blending polyetherimide, poly(arylene ether sulfone) or cyclic olefin copolymer with filler.
[0007] A method for preparing the composition, wherein the composition comprises a polyetherimide, comprising: contacting an aromatic bis(ether anhydride) and an organic amine to provide a polyetherimide precursor; combining a filler with the polyetherimide precursor to provide a mixture; and heating the mixture under conditions that effectively provide the corresponding polyetherimide.
[0008] An article comprising the composition.
[0009] The above and other features are illustrated by the following figures and detailed description. Attached Figure Description
[0010] The following figures are exemplary embodiments, in which the same elements are numbered the same.
[0011] Figure 1 These are scanning electron microscope (SEM) images of the composition according to Example 8.
[0012] Figure 2 These are scanning electron microscope (SEM) images of the composition according to Example 61.
[0013] Figure 3 These are scanning electron microscope (SEM) images of the composition according to Example 65. Detailed Implementation
[0014] The inventors have unexpectedly discovered that compositions comprising polyetherimide, poly(aryl ether sulfone), cyclic olefin copolymers, or combinations thereof, and specific inorganic fillers can provide a desired combination of properties. In particular, the compositions described herein can be formed into thin films by solution-based methods, exhibiting a low coefficient of thermal expansion (CTE), high infrared (IR) transmittance, and good processability. The compositions described herein are particularly suitable for a wide variety of articles, especially those for optical applications.
[0015] Therefore, this composition is one aspect of this disclosure. The composition comprises polyetherimide, poly(aryl ether sulfone), cyclic olefin copolymer, or a combination thereof.
[0016] In one aspect, the composition comprises a polyetherimide. The polyetherimide comprises more than 1, for example, 2 to 1000, or 5 to 500, or 10 to 100 structural units of formula (1).
[0017]
[0018] Each R is independently the same or different, and is a substituted or unsubstituted divalent organic group, such as a substituted or unsubstituted C. 6-20 Aromatic hydrocarbon groups, substituted or unsubstituted straight-chain or branched C4 groups 4-20 Alkylene, substituted or unsubstituted C 3-8 Cycloalkylene compounds, particularly halogenated derivatives of any of the foregoing. In one aspect, R is one or more divalent groups of formula (2):
[0019]
[0020] Among them, Q 1 Is -O-, -S-, -C(O)-, -SO2-, -SO-, -P(R a )(=O)-, where R a It is C 1-8 Alkyl or C 6-12 Aryl, -C y H 2y -, where y is an integer from 1 to 5 or a halogenated derivative thereof (which contains a perfluoroalkylene group), or -(C6H 10 ) z - where z is an integer from 1 to 4. In one aspect, R is m-phenylene, p-phenylene, or aryl sulfone, particularly bis(4,4'-phenylene) sulfone, bis(3,4'-phenylene) sulfone, bis(3,3'-phenylene) sulfone, or a combination comprising at least one of the foregoing. In one aspect, at least 10 mol% or at least 50 mol% of the R group contains a sulfone group, while in other aspects, no R group contains a sulfone group.
[0021] Further, in formula (1), T is a group of -O- or -OZO-, wherein the divalent bond of the -O- or -OZO- group is at the 3,3', 3,4', 4,3' or 4,4' position, and Z is optionally surrounded by 1 to 6 C atoms. 1-8 Alkyl groups, 1 to 8 halogen atoms, or aromatic C groups comprising at least one of the foregoing substituted groups. 6-24 Monocyclic or polycyclic moiety, provided that the valence of Z does not exceed that of Z. Exemplary group Z includes groups of formula (3):
[0022]
[0023] Among them, R a and R b Each is independently the same or different, and for example, a halogen atom or a monovalent carbon atom. 1-6 Alkyl group; p and q are each independent integers from 0 to 4; c is from 0 to 4; and X a It is a bridging group that connects a hydroxyl-substituted aromatic group, wherein the bridging group and the hydroxyl substituent of each C6 arylene are arranged ortho, meta, or para (especially para) to each other on the C6 arylene. Bridging group X a It can be a single bond, -O-, -S-, -S(O)-, -S(O)2-, -C(O)-, or C 1-18 Organic bridging base. C 1-18 The organic bridging group can be cyclic or acyclic, aromatic or non-aromatic, and can further contain heteroatoms such as halogens, oxygen, nitrogen, sulfur, silicon, or phosphorus. It can be arranged in C1... 1-18 The organic group causes each of the C6 arylene groups attached to it to be attached to a common alkylene carbon or to a C6 alkylene carbon. 1-18 Different carbon atoms in the organic bridging group. A specific example of group Z is the divalent group of formula (3a):
[0024]
[0025] Where Q is -O-, -S-, -C(O)-, -SO2-, -SO-, -P(R)- a )(=O)-, where R a It is C 1-8 Alkyl or C 6-12 Aryl or -C y H 2y - where y is an integer from 1 to 5 or a halogenated derivative thereof (including perfluoroalkylene). In one aspect, Z is derived from bisphenol A such that Q in formula (3a) is 2,2-isopropylene.
[0026] In one aspect, in formula (1), R is m-phenylene, p-phenylene, or a combination containing at least one of the foregoing, and T is -OZO-, wherein Z is a divalent group of formula (3a). Alternatively, R is m-phenylene, p-phenylene, or a combination containing at least one of the foregoing, and T is -OZO-, wherein Z is a divalent group of formula (3a), and Q is 2,2-isopropylene. Such materials are available from SABIC under the trade name ULTEM. Alternatively, the polyetherimide can be a copolymer comprising a polyetherimide unit of formula (1) of another structure, wherein at least 50 mol% of the R group is bis(4,4'-phenylene) sulfone, bis(3,4'-phenylene) sulfone, bis(3,3'-phenylene) sulfone, or a combination comprising at least one of the foregoing, and the remaining R group is p-phenylene, m-phenylene, or a combination comprising at least one of the foregoing; and Z is 2,2-(4-phenylene)isopropylene, i.e., the bisphenol A moiety, an example of which is commercially available from SABIC under the trade name EXTEM.
[0027] In one aspect, the polyetherimide is a copolymer that optionally contains additional structural imide units that are not polyetherimide units, such as the imide units of formula (4).
[0028]
[0029] Where R is as described in equation (1), each V is the same or different, and is a substituted or unsubstituted C. 6-20 Aromatic hydrocarbon groups, such as tetravalent linkages of the following formula:
[0030]
[0031] Where W represents a single bond, -O-, -S-, -C(O)-, -SO2-, -SO-, or C. 1-18 Hydroxyl group, -P(R) a )(=O)-, where R a It is C 1-8 Alkyl or C 6-12 aryl, or -C y H 2y - where y is an integer from 1 to 5 or a halogenated derivative thereof (including perfluoroalkylene). These additional structural imide units preferably comprise less than 20 mol% of the total number of units, and more preferably may be present in amounts of 0 mol% to 10 mol% of the total number of units, or 0 mol% to 5 mol% of the total number of units, or 0 mol% to 2 mol% of the total number of units. In one aspect, no additional imide units are present in the polyether imide.
[0032] Polyetherimides can be prepared by any method known to those skilled in the art, including the reaction of an aromatic bis(ether anhydride) of formula (5) or its chemical equivalent with an organic diamine of formula (6):
[0033]
[0034] Wherein, T and R are as defined above. Copolymers of polyetherimides can be prepared by using a combination of aromatic bis(ether anhydride) of formula (5) and other bis(anhydrides) that are not bis(ether anhydrides) (e.g., pyromellitic dianhydride or bis(3,4-dicarboxyphenyl)sulfone dianhydride).
[0035] Exemplary examples of aromatic bis(ether anhydrides) include 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (also known as bisphenol A dianhydride or BPADA), 3,3-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride; 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl ether dianhydride; 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl sulfide dianhydride; 4,4'-bis(3,4-dicarboxyphenoxy)benzophenone dianhydride; 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl sulfone dianhydride; 4,4'-bis(2,3-dicarboxyphenoxy)diphenyl ether dianhydride; 4,4'-bis(2,3-dicarboxyphenoxy)diphenyl sulfide dianhydride; 4,4'-bis(2,3-dicarboxyphenoxy)diphenyl sulfide dianhydride; 4,4'-bis(2,3-dicarboxyphenoxy)diphenylsulfone dianhydride; 4-(2,3-dicarboxyphenoxy)-4'-(3,4-dicarboxyphenoxy)diphenyl-2,2-propane dianhydride; 4-(2,3-dicarboxyphenoxy)-4'-(3,4-dicarboxyphenoxy)diphenyl ether dianhydride; 4-(2,3-dicarboxyphenoxy)-4'-(3,4-dicarboxyphenoxy)diphenyl sulfide dianhydride; 4-(2,3-dicarboxyphenoxy)-4'-(3,4-dicarboxyphenoxy)diphenyl ketone dianhydride; 4,4'-(hexafluoroisopropylidene)diphthalic anhydride; and 4-(2,3-dicarboxyphenoxy)-4'-(3,4-dicarboxyphenoxy)diphenylsulfone dianhydride. Different combinations of aromatic bis(ether anhydrides) can be used.
[0036] Examples of organic diamines include 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,12-dodecanediamine, 1,18-octadecanediamine, 3-methylheptamethyldiamine, 4,4-dimethylheptamethyldiamine, 4-methylnonamethylenediamine, 5-methylnonamethylenediamine, and 2,5-dimethyldiamine. 2,5-Dimethylheptamethyldiamine, 2,2-Dimethylpropanediamine, N-methyl-bis(3-aminopropyl)amine, 3-methoxyhexamethylenediamine, 1,2-bis(3-aminopropoxy)ethane, bis(3-aminopropyl)sulfide, 1,4-cyclohexanediamine, bis-(4-aminocyclohexyl)methane, m-phenylenediamine, p-phenylenediamine, 2,4-diaminotoluene, 2,6-diaminotoluene m-Phenylenedimethyldiamine, p-Phenylenedimethyldiamine, 2-Methyl-4,6-diethyl-1,3-phenylenediamine, 5-Methyl-4,6-diethyl-1,3-phenylene-diamine, benzidine, 3,3'-dimethylbenzidine, 3,3'-dimethoxybenzidine, 1,5-diaminonaphthalene, bis(4-aminophenyl)methane, bis(2-chloro-4-amino-3,5-diethylphenyl)methane, bis(4-amino... 2,4-Bis(p-amino-tert-butyl)toluene, bis(p-amino-tert-butylphenyl) ether, bis(p-methyl-o-aminophenyl)benzene, bis(p-methyl-o-aminopentyl)benzene, 1,3-diamino-4-isopropylbenzene, bis(4-aminophenyl) sulfide, bis-(4-aminophenyl) sulfone (also known as 4,4'-diaminodiphenyl sulfone (DDS)), and bis(4-aminophenyl) ether. Any regiomeric isomers of the aforementioned compounds may be used. Any of the aforementioned C-type compounds may be used. 1-4 Alkylated or poly(C) 1-4 Alkylated derivatives, such as a polymethylated 1,6-hexanediamine. Combinations of these compounds may also be used. In one aspect, the organic diamine is m-phenylenediamine, p-phenylenediamine, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, or a combination comprising at least one of the foregoing. In another aspect, the organic diamine is m-phenylenediamine, p-phenylenediamine, or a combination thereof, preferably m-phenylene.
[0037] Polyetherimides can have a melt index of 0.1 g / min to 10 g / min, measured at 340°C to 370°C using a 6.7 kg weight, according to ASTM D1238. In one aspect, polyetherimides have a weight-average molecular weight (Mw) of 1,000 to 150,000 g / mol (or Daltons (Da)) determined using polystyrene standards by gel permeation chromatography. In another aspect, polyetherimides have a Mw of 10,000 to 80,000 g / mol. These types of polyetherimides typically have an intrinsic viscosity greater than 0.2 dL / g, or more specifically, 0.35 dL / g to 0.7 dL / g, measured in m-cresol at 25°C.
[0038] In one aspect, the composition comprises poly(aryl ether sulfone). As used herein, the term "poly(aryl ether sulfone)" may refer to a polymer having repeating units of formula (7):
[0039] -Ar 1 -SO2-Ar 2 -O-(7)
[0040] Among them, Ar 1 and Ar 2 Each group may be the same or different, and is a group of formula (8):
[0041]
[0042] Where c is 0 or 1, R a and R b Each is independently either a straight chain or a branched chain C. 1-10 Alkyl, straight-chain or branched C 2-10 Alkenyl, straight-chain or branched C 2-10 alkynyl group, C 6-18 Aryl, C 7-20 Alkyl, C 7-20 Aryl alkyl, C 5-10 cycloalkyl, C 5-20 Cycloalkenyl, straight-chain or branched C 1-10 alkyl carbonyl, C 6-18 Aryl carbonyl, halogen, nitro, cyano, halogen, C 1-12 alkoxy, or C 1-12 Alkyl groups, and p and q are each independent integers from 0 to 4. It should be understood that when p or q is less than 4, the valence of each carbon in the ring is filled with hydrogen. Also in equation (8), X aIt is a bridging group that connects two hydroxyl-substituted aromatic groups, wherein the bridging group and the hydroxyl substituents of each C6 arylene are arranged ortho, meta, or para (especially para) to each other on the C6 arylene. In one aspect, the bridging group X a It is a single bond, -O-, -S-, -S(O)-, -S(O) 2- -C(O)- or C 1-18 Organic groups. C 1-18 The organic bridging group can be cyclic or acyclic, aromatic or non-aromatic, and can further contain heteroatoms such as halogens, oxygen, nitrogen, sulfur, silicon, or phosphorus. It can be arranged in C1... 1-18 The organic group causes each of the C6 arylene groups attached to it to be attached to a common alkylene carbon or to a C6 alkylene carbon. 1-18 Different carbon atoms in an organic bridging group. In one aspect, c is 0 or 1, p and q are each 0, and X a It is isopropylidene.
[0043] Specific poly(arylene ether sulfone) that can be used includes polyether sulfone (also known as "PES" or "PESU"), which contains at least 85 wt% of units of formula (8a).
[0044]
[0045] Or polyphenylsulfone (also known as "PPSU" or polyphenylene sulfone), which contains at least 85 wt% of units of formula (8b):
[0046]
[0047] Or polyether ether sulfone, which contains at least 85% by weight of units having formula (8c).
[0048]
[0049] Or polysulfone (commonly referred to as "PSU"), which contains at least 85 wt% of units of formula (8d).
[0050]
[0051] Or a combination comprising at least one of the aforementioned poly(arylene ether sulfone). Copolymers comprising combinations of units of at least two types of formulas (8a), (8b), (8c), and (8d) may also be used.
[0052] Poly(aryl ether sulfone) can be linear or branched, having one or more, two or more, or five or more branching points per 1,000 carbon atoms along the polymer chain. In one aspect, poly(aryl ether sulfone) is linear, having 10 or fewer, five or fewer, two or fewer, or one or fewer branching points per 1,000 carbon atoms along the polymer chain. In another aspect, poly(aryl ether sulfone) has a glass transition temperature (Tg) greater than 175°C, particularly greater than 175°C to 300°C, or 200°C to 280°C, or 255°C to 275°C. Poly(arylene ether sulfone) may further have a weight-average molecular weight (Mw) of 500 g / mol to 100,000 g / mol, especially 1,000 g / mol to 75,000 g / mol, more especially 1,500 g / mol to 50,000 g / mol, and even more especially 2,000 g / mol to 25,000 g / mol.
[0053] Exemplary poly(arylene ether sulfone) that can be used include those available from sources such as Solvay Specialty Polymers, Quadrant EPP, Centroplast Centro, Duneon, GEHR Plastics, Westlake Plastics, Gharda Chemicals, Sumitomo Chemical, and UJU New Materials Co., Ltd. Commercial-grade poly(phenyl sulfone) includes those with the trade name RADEL. TM UDEL TM ULTRASON TM GAFONE TM and PARYLS TM Those. Poly(arylene ether sulfone) is from Solvay Advanced Polymers KK in Veradel. TM Commercially available products under the trademark of BASF Corporation in ULTRASON TM Commercially available under the trademark and from Sumitomo Chemical Co., Ltd. in SUMIKA EXCEL TM It is available for commercial purchase under the trademark.
[0054] Polyphenylsulfone (PPS) is commercially available and comprises the condensation product of bisphenol and dichlorodiphenyl sulfone. Methods for preparing PPS are well known, and several suitable methods have been well described in the art. The carbonate method and the alkali metal hydroxide method are both known to those skilled in the art. In the alkali metal hydroxide method, a dialkali metal salt of a bisphenol is contacted with a dihalophenyl ring compound under substantially anhydrous conditions in the presence of a dipolar aprotic solvent. A carbonate method is also disclosed in the art, wherein the bisphenol and the dihalophenyl ring compound are heated together with, for example, sodium carbonate or sodium bicarbonate and a second alkali metal carbonate or bicarbonate, as described, for example in U.S. Patent No. 4,176,222. Alternatively, the PPS can be prepared by any of a variety of methods known in the art.
[0055] As shown by reduced viscosity data in suitable solvents (such as dichloromethane, chloroform, N-methylpyrrolidone, etc.), the molecular weight of polyphenylsulfone can be greater than or equal to 0.3 dl / g, or more specifically, greater than or equal to 0.4 dl / g, and will generally not exceed 1.5 dl / g.
[0056] When polystyrene standards are used and determined by gel permeation chromatography according to ASTM D5296, the weight-average molecular weight (Mw) of polyphenylene sulfone can be from 10,000 g / mol to 100,000 g / mol. In one aspect, the weight-average molecular weight of polyphenylene sulfone can be from 10,000 g / mol to 80,000 g / mol. Polyphenylene sulfone can have a glass transition temperature (Tg) from 180 °C to 250 °C, as determined by differential scanning calorimetry (DSC).
[0057] In one aspect, the composition comprises a cyclic olefin copolymer. The cyclic olefin copolymer is derived from the copolymerization of cyclic olefins. Examples of suitable cyclic olefin monomers are norbornene, tetracyclododecene, bicyclo[2,2,1]hept-2-ene, 1-methylbicyclo[2,2,1]hept-2-ene, and hexacyclo[6,6,1,1]hept-2-ene. 3 ,6,1 10 ,13,0 2 ,7,0 9
[14] -4-heptadecene and combinations thereof. Many such monomers are well known and described, for example, in U.S. Patent No. 5,008,356. In the case of cyclic olefin copolymers (COCs), one or more comonomers are selected from a variety of suitable olefins, including, for example, acyclic olefins. Many such comonomers are also well known in the literature, including, for example, the aforementioned U.S. Patent No. 5,008,356. In one aspect, the cyclic olefin monomers include norbornene, and the comonomers include acyclic olefins, such as ethylene, propylene, etc.
[0058] In one respect, polyetherimide, poly(aryl ether sulfone), cycloolefin comonomer, or combinations thereof can have a transmittance greater than 70% from 850 nm to 1100 nm and from 1200 nm to 1330 nm, as determined using UV / Vis spectroscopy, and for example, a thickness of 100 micrometers.
[0059] Based on the total weight of the composition, polyetherimide, poly(aryl ether sulfone), cyclic olefin copolymers, or combinations thereof may be present in the composition in an amount greater than 50 wt% to less than 75 wt%. Within this range, polyetherimide, poly(aryl ether sulfone), cyclic olefin copolymers, or combinations thereof may be present in an amount of 53 to 72 wt%, or 53 to 70 wt%, or 53 to 68 wt%, or 55 to 65 wt%, or 58 to 62 wt%.
[0060] In addition to polyetherimide, poly(aryl ether sulfone), cyclic olefin copolyamide, or combinations thereof, the composition further comprises a filler. The filler may preferably have a refractive index of 1.60 to 1.68, 1.60 to 1.67, or 1.60 to 1.66 as measured at a wavelength of 587 nm. The filler comprises boehmite, wollastonite, or combinations thereof, and each may optionally be surface modified. In one aspect, the filler does not include any surface modification. As further described in the working examples below, the selection of the filler may depend on the polymer present in the composition (e.g., polyetherimide, poly(aryl ether sulfone), or cyclic olefin copolymer). Depending on the polymer present in the composition, the filler may be further selected based on average particle size, surface area, bulk density, or one or more of the composition. Average particle size can be determined by a variety of methods generally known, including laser scattering techniques or microscopy, such as scanning electron microscopy. Surface area may refer to the Brunauer–Emmett–Teller (BET) specific surface area as determined according to ISO 9277. Bulk density can refer to the loose bulk density of filler and can be determined by commonly known methods, such as according to ASTM D7481-18.
[0061] In one aspect, the filler may include wollastonite fibers. In one aspect, the wollastonite fibers may have an average fiber diameter of 5 to 10 micrometers and an average fiber length of 55 to 75 micrometers. In one aspect, the wollastonite fibers may have an average fiber diameter of 1 to 5 micrometers and an average fiber length of 5 to 12 micrometers. In one aspect, the wollastonite fibers may have an average fiber diameter of 10 to 15 micrometers and an average fiber length of 140 to 165 micrometers.
[0062] In one aspect, the composition comprises a polyetherimide and a filler comprising an average fiber diameter of 5 to 10 micrometers and an average fiber length of 55 to 75 micrometers, and a fiber length of 2.5 m.2 / g to less than 2.9m 2 Wollastonite fibers with a surface area of / g, a bulk density of 0.42g / cc to 0.50g / cc, and a silica content of 52% to 55%.
[0063] In one aspect, the composition comprises poly(aryl ether sulfone) and the filler comprises an average fiber diameter of 1 micrometer to 5 micrometers and an average fiber length of 5 micrometers to 12 micrometers, 3.8m 2 / g to 4.3m 2 Wollastonite fibers with a surface area of / g and a bulk density of 0.48g / cc to 0.56g / cc.
[0064] In one aspect, the composition comprises a cyclic olefin copolymer and the filler comprises an average fiber diameter of 10 to 15 micrometers and an average fiber length of 140 to 165 micrometers, with a thickness of 1.0 m. 2 / g to 1.8m 2 Wollastonite fibers with a surface area of / g and a bulk density of 0.18g / cc to 0.26g / cc.
[0065] In one aspect, the filler may include boehmite (also known as alumina hydroxide). Boehmite preferably has a refractive index of 1.60 to 1.68, 1.60 to 1.67, or 1.60 to 1.66 as measured at a wavelength of 587 nm. Inorganic fillers may have an average particle size of 0.4 μm to less than 0.9 μm as measured by laser scattering.
[0066] In one aspect, the composition comprises polyetherimide, and the filler comprises boehmite having an average particle size (D50) of 0.4 micrometers to less than 0.9 micrometers as determined by laser scattering.
[0067] In one aspect, the composition comprises poly(arylene ether sulfone), and the filler comprises boehmite having an average particle size (D50) of 0.4 micrometers to less than 0.9 micrometers as determined by laser scattering.
[0068] In one aspect, the composition comprises a cyclic olefin copolymer, and the filler does not include boehmite.
[0069] Based on the total weight of the composition, the filler may be included in the composition in an amount greater than 25 wt% to less than 50 wt%. Within this range, the filler may be present in an amount of 28 wt% to 48 wt%, or 30 wt% to 48 wt%, or 32 wt% to 47 wt%, or 35 wt% to 45 wt%, or 38 wt% to 42 wt%.
[0070] In one aspect, the composition comprises a polyetherimide, poly(aryl ether sulfone), a cyclic olefin copolymer, or a combination thereof, and a filler, substantially consisting of a polyetherimide, poly(aryl ether sulfone), a cyclic olefin copolymer, or a combination thereof, and a filler, or consisting of a polyetherimide, poly(aryl ether sulfone), a cyclic olefin copolymer, or a combination thereof, and a filler. In one aspect, the composition may exclude any component other than a polyetherimide, poly(aryl ether sulfone), a cyclic olefin polymer, or a combination thereof, and a filler not specifically described herein. In one aspect, the composition comprises less than 5 wt%, or less than 1 wt% (based on the total weight of the composition), of any thermoplastic polymer other than a polyetherimide, poly(aryl ether sulfone), and a cyclic olefin copolymer. The composition may optionally exclude any inorganic filler other than boehmite or wollastonite.
[0071] In one aspect, the composition may optionally further comprise an additive composition, comprising one or more additives selected to achieve the desired properties, provided that the additives are also selected so as not to significantly adversely affect the desired properties of the composition. During the mixing of the components used to form the composition, the additive composition or individual additives may be mixed at appropriate times. The additive composition may comprise impact modifiers, flow modifiers, fillers (e.g., particulate polytetrafluoroethylene (PTFE), glass, carbon, minerals, or metals), reinforcing agents (e.g., glass fibers), antioxidants, heat stabilizers, light stabilizers, ultraviolet (UV) light stabilizers, UV absorbing additives, plasticizers, lubricants, mold release agents (such as release agents), antistatic agents, antifogging agents, antimicrobial agents, colorants (e.g., dyes or pigments), surface effect additives, radiation stabilizers, flame retardants, anti-dripping agents (e.g., PTFE-encapsulated styrene-acrylonitrile copolymer (TSAN)), or combinations thereof. For example, a combination of heat stabilizers, mold release agents, and UV light stabilizers may be used. Generally, additives are used in amounts that are generally known to be effective. For example, the total amount of the additive composition (other than any impact modifier, filler, or reinforcing agent) may be from 0.001 wt% to 10.0 wt% or from 0.01 wt% to 5 wt%, each based on the total weight of the composition.
[0072] In one aspect, the composition may further comprise an additive composition comprising an antioxidant, a heat stabilizer, a water stabilizer, a UV stabilizer, a release agent, or a combination comprising at least one of the foregoing.
[0073] The composition can be prepared by various methods commonly known in the art. For example, polyetherimide, poly(aryl ether sulfone), cyclic olefin copolymers, or combinations thereof can be blended with filler, for example in a high-speed mixer or by manual mixing. In one aspect, the components of the blended composition may preferably be in the presence of a solvent. Any organic solvent capable of solubilizing the components of the composition can be used, such as o-dichlorobenzene, dichloromethane, N-methylpyrrolidone, dimethyl, or acetamide. The components combined in the solvent can be mixed to disperse the filler over a suitable time (e.g., 1 hour to 10 hours). The method for preparing the composition is further illustrated in the following working examples.
[0074] The components of the composition can be blended at a temperature of 20°C to 200°C, preferably 20°C to 25°C or 175°C to 200°C.
[0075] In one aspect, the composition can be prepared by contacting an aromatic bis(ether anhydride) and an organic amine to provide a polyetherimide precursor and combining a filler with the polyetherimide precursor to provide a mixture. The mixture can be heated under conditions that effectively provide the corresponding polyetherimide (i.e., promote the imidization of the precursor).
[0076] The composition can be further formed into a film, for example using various commonly known coating techniques, including solution coating, spin coating, blade coating, droplet casting, etc. The solvent can be removed from the film. The film thickness can be, for example, 50 micrometers to 500 micrometers, or 50 micrometers to 250 micrometers, or 50 micrometers to 150 micrometers, or 75 micrometers to 125 micrometers.
[0077] The film formed from this composition can exhibit one or more advantageous properties. For example, according to ASTM E831, the film formed from the composition can exhibit a coefficient of thermal expansion of less than or equal to 36 ppm / °C, or from 5 ppm / °C to 36 ppm / °C. The film formed from this composition can exhibit a percentage transmittance of greater than 50%, or greater than 50% to 95%, at 1330 nm with a thickness of 100 μm. The transmittance of the film can be determined by UV / Vis spectroscopy using a Perkin Elmer Lambda 950 spectrometer with an integrating sphere for measuring transmittance at a set wavelength of 1330 nm. In one aspect, the film formed from the composition can exhibit both of the aforementioned properties.
[0078] In one aspect, the composition comprises polyetherimide and the filler comprises wollastonite, and the film formed from the composition exhibits a coefficient of thermal expansion of less than or equal to 25 ppm / °C, or from 5 ppm / °C to 25 ppm / °C, as determined according to ASTM D256; and a transmittance percentage of greater than 50%, or from 50% to 95%, at 1330 nm, as determined by UV / Vis spectroscopy at a thickness of 100 μm.
[0079] In one aspect, the composition comprises polyetherimide and the filler comprises boehmite, and the film formed from the composition exhibits a coefficient of thermal expansion of less than or equal to 35 ppm / °C, or from 5 ppm / °C to 35 ppm / °C, as determined according to ASTM D256; and a percentage transmittance of greater than 75%, or from 75% to 95%, at 1330 nm, as determined by UV / Vis spectroscopy at a thickness of 100 μm.
[0080] In one aspect, the composition comprises poly(arylene ether sulfone) and the filler comprises wollastonite, and the film formed from the composition exhibits a coefficient of thermal expansion of less than or equal to 36 ppm / °C, or from 5 ppm / °C to 36 ppm / °C, as determined according to ASTM E831; and a transmittance percentage of greater than 50%, or from 50% to 95%, at 1330 nm at a thickness of 100 μm, as determined by UV / Vis spectroscopy.
[0081] In one aspect, the composition comprises poly(arylene ether sulfone) and the filler comprises boehmite, and the film formed from the composition exhibits a coefficient of thermal expansion of less than or equal to 35 ppm / °C or from 5 ppm / °C to 35 ppm / °C as determined according to ASTM E831; and a transmittance percentage of greater than 50% or greater than 50% to 95% at 1330 nm as determined by UV / Vis spectroscopy at a thickness of 100 micrometers.
[0082] In one aspect, the composition comprises a cyclic olefin copolymer and the filler comprises wollastonite, and the film formed from the composition exhibits a coefficient of thermal expansion of less than or equal to 35 ppm / °C, or from 5 ppm / °C to 35 ppm / °C, as determined according to ASTM E831; and a transmittance percentage of greater than 50%, or from 50% to 95%, at 1330 nm, as determined by UV / Vis spectroscopy at a thickness of 100 micrometers.
[0083] Articles comprising the composition represent another aspect of this disclosure. For example, articles can be prepared by molding, extruding, or forming the above-described composition into articles. The composition can be molded into useful molded articles by various methods such as injection molding, extrusion, rotational molding, blow molding, and thermoforming. Exemplary articles may be in the form of fibers, films, sheets, tubes, or molded parts. The physical properties of the compositions described herein can provide articles particularly suitable for use in transparent articles (e.g., for optical applications). Such articles may include optical articles, preferably optical lenses, lens arrays, and transparent materials used in medical devices, electronics and telecommunications, architecture and structures, sensors, antennas, electrodes, thin-film optics, thin-film substrates, transistors, and IR transparent display devices. In one aspect, the article may be a lens for a single-mode fiber optic connector.
[0084] This disclosure is further illustrated by the following examples, which are non-limiting.
[0085] Example
[0086] The materials used in the following embodiments are described in Table 1.
[0087] Table 1
[0088]
[0089]
[0090] The compositions were prepared by solution blending of the polymer and filler according to the compositions described in Table 2. The amount of each component is provided as a weight percentage based on the total weight of the composition. Specifically, the compositions were prepared using one of three methods: 1) dissolving the polymer in a solvent (PEI and DCM) at room temperature, followed by the addition of the filler. The resulting solution was stirred with a mechanical stirrer / shaker to disperse the filler in the resin for 5–7 hours; 2) dissolving the polymer in a solvent (PEI with oDCB; PPSU with NMP; PES with DMAc; and COC in oDCB), followed by the addition of the filler. In this method, 300 mL of dry oDCB was added to PEI in a four-necked round-bottom flask equipped with a mechanical stirrer, nitrogen inlet, thermocouple sheath (thermowell), and a Dean-Stark apparatus with a reflux condenser. The flask was purged with nitrogen and then heated to 210°C (oil bath temperature) to remove trace amounts of moisture using the Dean-Stark apparatus. The temperature inside the flask was 180°C. After 90 minutes, PEI was completely dissolved in oDCB to form a clear solution. The packing material was added, followed by 50 mL of additional oDCB. The resulting mixture was allowed to be stirred at 180°C for 7–9 hours to complete dispersion; and 3) in a four-necked round-bottom flask equipped with a mechanical stirrer, nitrogen inlet, thermocouple sheath, and a Dean-Stark apparatus with a reflux condenser, 41 g of dried oDCB was added to bisphenol A dianhydride (BPADA). The flask was purged with nitrogen and then heated to 210°C (oil bath temperature) to remove trace amounts of moisture through the Dean-Stark apparatus. The temperature inside the flask was 180°C. After 90 minutes, BPADA was completely dissolved in oDCB to form a clear solution. The reaction mixture was allowed to cool to 90°C and 8.6 g of m-phenylenediamine was added to the mixture. The flask was heated to 210°C (oil bath temperature) while maintaining the internal temperature at 180°C. The reaction mixture was stirred for 90 minutes to obtain a clear, yellow, viscous solution of polyamic acid (PAA). The filler was added, followed by 50 mL of additional oDCB. The filler was mixed with the polyamic acid to form a filler-PAA mixture. The mixture was stirred at 180°C for 7–9 hours to complete polymerization and form the corresponding polyetherimide.
[0091] Regardless of the processing method used, a coating blade was used to spread the polymer solution onto a glass plate in the longitudinal flow direction to control the film thickness. The film was then held in a fume hood for 24 hours and peeled off from the glass plate. The film was cut and heat-dried under vacuum at 120–180°C for 24 hours to remove the solvent. The film was cooled to room temperature and its thermal and optical properties were tested. The film thickness was 100 micrometers.
[0092] Performance was measured using ASTM testing methods. All membrane samples were conditioned at 50% relative humidity for at least 48 hours prior to testing.
[0093] Thermal expansion (CTE) measurements were performed according to ASTM E831 using a DuPont 2940 probe at a heating rate of 58 °C / min, with a tension of 0.05 N on the film. CTE values were recorded on a temperature scale between 30 °C and 80 °C.
[0094] According to ASTM E 1131, thermogravimetric analysis (TGA) was performed on the membrane at a heating rate of 10°C / min using a Q 5000-TA Instruments to determine the filler content within the range of 25°C to 1000°C.
[0095] Percentage transmittance was measured in the IR region using a Perkin Elmer Lambda 900 UV-Vis spectrophotometer with an integrating sphere and a 2-nanometer slit width.
[0096] Haze was measured in the visible region (i.e., 400 nm to 750 nm) using a haze meter (Haze-gard from BYK-Gardner) according to ASTM D1003 standard. Percentage haze is expressed as diffuse transmittance T. d With total light transmittance T t The ratio is calculated as follows:
[0097] Haze, % = T d / T t *100)
[0098] The compositions in Table 2 were prepared using method 1 as described above.
[0099] Table 2a
[0100]
[0101]
[0102] * indicates a comparison example.
[0103] Table 2b
[0104]
[0105]
[0106] * indicates a comparison example.
[0107] Table 2c
[0108]
[0109]
[0110] * indicates a comparison example.
[0111] Table 2d
[0112]
[0113]
[0114] The compositions in Table 3 were prepared using method 2 as described above.
[0115] Table 3a
[0116]
[0117]
[0118] Table 3b
[0119]
[0120]
[0121] * indicates a comparison example.
[0122] Examples 1-5 demonstrate the effect of different types of fillers in the PEI compositions. The compositions for each of these examples were prepared according to method (1) described above. Example 1 shows that using wollastonite 1 in a specific amount provides a composition capable of achieving a percentage transmittance greater than or equal to 50 at 1330 nm and a CTE less than 25 ppm / °C. Example 5 shows that using a specific amount of boehmite filler provides a composition capable of achieving a percentage transmittance greater than or equal to 75 at 1330 nm and a CTE less than 35 ppm / °C.
[0123] Examples 6-9 demonstrate that the particle size of the filler can affect the resulting PEI compositions. The compositions for each of these examples were prepared according to method (1) described above. In particular, these examples show that by using specific amounts of certain wollastonite fillers, compositions were produced that achieved a combination of percentage transmittance greater than or equal to 50 at 1330 nm and CTE less than 25 ppm / °C. It is anticipated that a lower particle size of the wollastonite filler would enhance both CTE and %T performance due to the dilution effect and the same mineral composition. However, only the composition containing wollastonite 4 showed an improvement in %T performance at 1330 nm compared to other wollastonite fillers.
[0124] Similarly, Examples 10-13 demonstrate that compositions with a combined percentage transmittance of greater than or equal to 75% at 1330 nm and a CTE of less than 35 ppm / °C can be obtained by using specific amounts of certain boehmite fillers. Due to the dilution effect and the same mineral composition, the lower particle size of the boehmite filler is expected to enhance both CTE and %T performance. However, only compositions containing AlO(OH)-4 showed improved %T performance at 1330 nm compared to other boehmite fillers.
[0125] Examples 14-17 and 22-29 show that a specific amount and size distribution of wollastonite are required to achieve the desired combination of a percentage transmittance of greater than or equal to 50% at 1330 nm and a CTE of less than 25 ppm / °C.
[0126] Examples 18-21 and 30-41 show that a specific amount of boehmite is required to achieve the desired combination of a percentage transmittance of greater than or equal to 75% at 1330 nm and a CTE of less than 35 ppm / °C.
[0127] The results shown in Table 2 are unexpected, as the refractive index of each filler is close to that of PEI; however, as indicated by the CTE and %T in Table 2, each filler does not provide the same effect on the properties of the resulting compositions. Furthermore, fillers such as kaolin and calcium carbonate do not exhibit the desired CTE and %T compared to wollastonite or boehmite. The examples shown in Table 2 clearly demonstrate that the desired CTE and %T are only obtained when specific combinations of PEI and wollastonite or boehmite are used, and further, when the fillers have specific particle sizes. No similar improvement in CTE and %T was observed when using lower or higher particle sizes.
[0128] The data shown in Tables 2 and 3 illustrate several factors that influence the choice of polymer and filler combination. More specifically, different types of fillers can provide different results depending on the choice of polyetherimide, poly(aryl ether sulfone), or cycloolefin copolymer. Without being bound by theory, these polymers each have different chemical compositions and structures, which can lead to different zeta potentials, hydrophilic / hydrophobic balances, and end-group interactions, each of which can affect the stability of the resulting composition. Therefore, without being bound by theory, it is believed that polymer / filler interaction energy, polymer swelling behavior, chain entanglement density, surface energy, the degree of polymer solvation, and polymer viscosity in the presence of filler can each influence the properties of the composition (particularly optical properties such as haze and transmittance, and thermal properties such as coefficient of thermal expansion).
[0129] The following examples illustrate the effects of the method for preparing the composition. The composition was prepared according to the method shown in Table 4.
[0130] Table 4
[0131]
[0132]
[0133] * indicates a comparison example.
[0134] Examples 61-67 and comparisons of those prepared by method 1 with similar compositions in Table 2 demonstrate that certain compositions with specific particle sizes and processing methods produce desired properties regarding CTE and %T. It was also observed that using method 2 or 3 provided enhanced dispersion and distribution of the filler in the composition compared to method 1. This can be observed by scanning electron microscopy, for example, as shown in... Figure 1 (SEM of Example 8) Figure 2 (SEM of Example 61) and Figure 3 (SEM of Example 65) is shown. Similar results were obtained when boehmite packing was used, as shown in Examples 68-71 in Table 4.
[0135] The present invention further covers the following aspects.
[0136] Aspect 1: A composition comprising greater than 50 wt% to less than 75 wt% of a polyetherimide, poly(aryl ether sulfone), or cyclic olefin copolymer; and greater than 25 wt% to less than 50 wt% of a filler; wherein, when the polymer comprises a polyetherimide, the filler comprises having an average fiber diameter of 5 micrometers to 10 micrometers and an average fiber length of 55 micrometers to 75 micrometers, and a fiber diameter of 2.5 m. 2 / g to less than 2.9m 2 Wollastonite fibers with a surface area of / g, a bulk density of 0.42g / cc to 0.50g / cc, and a silica content of 52% to 55%; or boehmite having an average particle size (D50) of 0.4 μm to less than 0.9 μm as determined by laser scattering; when the polymer includes poly(arylene ether sulfone), the filler comprises fibers with an average fiber diameter of 1 μm to 5 μm and an average fiber length of 5 μm to 12 μm, and a surface area of / g. 2 / g to 4.3m 2 Wollastonite fibers with a surface area of / g and a bulk density of 0.48g / cc to 0.56g / cc; or boehmite having an average particle size (D50) of 0.4 μm to less than 0.9 μm as determined by laser scattering; and when the polymer includes a cyclic olefin copolymer, the filler includes fibers with an average fiber diameter of 10 μm to 15 μm and an average fiber length of 140 μm to 165 μm, 1.0m 2 / g to 1.8m 2 / g surface area and 0.18g / cc to 0.26g / cc bulk density of wollastonite fibers; wherein, weight percentage is based on the total weight of the composition.
[0137] Aspect 2: The composition according to aspect 1, a flow thermal expansion coefficient less than or equal to 36 ppm / ℃ or 5 ppm / ℃ to 36 ppm / ℃ as determined by ASTM E831; and a transmittance percentage greater than 50% or greater than 50% to 95% at 1330 nm as determined by UV / Vis spectroscopy at a thickness of 100 micrometers.
[0138] Aspect 3: The composition according to aspect 1 or 2 comprises 53 wt% to 68 wt%, or 55 wt% to 65 wt%, or 58 wt% to 62 wt% of polyetherimide, poly(arylene ether sulfone), cyclic olefin copolymer or combinations thereof; and 32 wt% to 47 wt%, or 35 wt% to 45 wt%, or 38 wt% to 42 wt% of filler.
[0139] Aspect 4: The composition according to any one of Aspects 1 to 3, wherein polyetherimide is present and the filler comprises wollastonite, wherein the film formed from the composition exhibits a coefficient of thermal expansion of less than or equal to 25 ppm / °C, or from 5 ppm / °C to 25 ppm / °C, as determined according to ASTM D256; and a transmittance percentage of greater than 50%, or from greater than 50% to 95%, at 1330 nm, as determined by UV / Vis spectroscopy at a thickness of 100 μm.
[0140] Aspect 5: A composition according to any one of Aspects 1 to 3, wherein polyetherimide is present and the filler comprises boehmite, wherein the film formed from the composition exhibits a coefficient of thermal expansion of less than or equal to 35 ppm / °C, or from 5 ppm / °C to 35 ppm / °C, as determined according to ASTM D256; and a percentage transmittance of greater than 75%, or from greater than 75% to 95%, at 1330 nm, as determined by UV / Vis spectroscopy at a thickness of 100 μm.
[0141] Aspect 6: A composition according to any one of Aspects 1 to 3, wherein the poly(arylene ether sulfone) is present and the filler comprises the wollastonite, wherein the film formed from the composition exhibits a coefficient of thermal expansion of less than or equal to 36 ppm / °C, or from 5 ppm / °C to 36 ppm / °C, as determined according to ASTM E831; and a transmittance percentage of greater than 50%, or from greater than 50% to 95%, at 1330 nm, as determined by UV / Vis spectroscopy at a thickness of 100 micrometers.
[0142] Aspect 7: A composition according to any one of Aspects 1 to 3, wherein poly(arylene ether sulfone) is present and the filler comprises boehmite, wherein the film formed from the composition exhibits a coefficient of thermal expansion of less than or equal to 35 ppm / °C, or from 5 ppm / °C to 35 ppm / °C, as determined according to ASTM E831; and a transmittance percentage of greater than 50%, or from 50% to 95%, at 1330 nm at a thickness of 100 micrometers, as determined by UV / Vis spectroscopy.
[0143] Aspect 8: The composition according to any one of Aspects 1 to 3, wherein the cyclic olefin copolymer is present and the filler comprises the wollastonite, wherein the film formed from the composition exhibits a coefficient of thermal expansion of less than or equal to 35 ppm / °C, or from 5 ppm / °C to 35 ppm / °C, as determined according to ASTM E831; and a transmittance percentage of greater than 50%, or from 50% to 95%, at 1330 nm, as determined by UV / Vis spectroscopy at a thickness of 100 micrometers.
[0144] Aspect 9: A method of manufacturing a composition according to any one of Aspects 1 to 8, the method comprising: blending a polyetherimide, a poly(aryl ether sulfone), or a cyclic olefin copolymer with a filler.
[0145] Aspect 10: According to the method of aspect 9, wherein polyetherimide, poly(aryl ether sulfone) or cyclic olefin copolymer and filler are blended in the presence of a solvent.
[0146] Aspect 11: The method according to aspect 9 or 10, wherein the polyetherimide, poly(arylene ether sulfone), or cyclic olefin copolymer is blended at a temperature of 20°C to 200°C, preferably 20°C to 25°C or 175°C to 200°C.
[0147] Aspect 12: A method of manufacturing a composition according to any one of Aspects 1 to 8, wherein the composition comprises a polyetherimide, the method comprising: contacting an aromatic bis(ether anhydride) and an organic amine to provide a polyetherimide precursor; combining a filler with the polyetherimide precursor to provide a mixture; and heating the mixture under conditions that effectively provide the respective polyetherimide.
[0148] Aspect 13: An article comprising the composition according to any one of aspects 1 to 8.
[0149] Aspect 14: Articles of manufacture according to aspect 13, wherein the article is an optical article, preferably an optical lens, lens array, or transparent material, used in medical devices, electronics and telecommunications, architecture and structures, sensors, antennas, electrodes, thin-film optics, thin-film substrates, transistors, and IR transparent display devices.
[0150] Alternatively, compositions, methods, and articles may comprise, consist of, or consist substantially of any suitable materials, steps, or components disclosed herein. Compositions, methods, and articles may additionally, or alternatively, be formulated to be free of, or substantially free of, any materials (or species), steps, or components that would otherwise be unnecessary for achieving the function or purpose of the composition, method, and article.
[0151] All scopes disclosed herein include endpoints, and endpoints may be combined independently of each other. "Combination" includes blends, mixtures, alloys, reaction products, etc. The terms "first," "second," etc., do not indicate any order, quantity, or importance, but are used to distinguish one element from another. Unless otherwise stated herein or clearly contradicted by the context, the terms "an," "a," and "the" do not indicate a limitation of quantity, but are interpreted to cover both singular and plural. Unless otherwise expressly stated, "or" means "and / or." Throughout the specification, reference to "an aspect" means that a particular element described in connection with that aspect is included in at least one aspect described herein and may or may not be present in other aspects. The term "combination of them," as used herein, includes one or more listed elements and is open to the presence of one or more unnamed similar elements. Furthermore, it should be understood that the described elements may be combined in any suitable manner in each aspect.
[0152] Unless otherwise specified herein, all test standards are the most recent standards effective from the filing date of this application, or, if priority is claimed, the filing date of the earliest priority application in which the test standard appears.
[0153] Unless otherwise defined, the technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains. All cited patents, patent applications, and other references are incorporated herein by reference in their entirety. However, if any terminology in this application contradicts or conflicts with terminology in the incorporated references, the terminology from this application shall take precedence over the conflicting terminology from the incorporated references.
[0154] Compounds should be described using standard nomenclature. For example, any position not substituted by any indicator group should be understood as having its valence filled by a bond or hydrogen atom as indicated. A dash ("-") not between two letters or symbols is used to indicate the connection point of a substituent. For example, -CHO is connected through the carbonyl group.
[0155] As used herein, the term "alkyl group," whether used alone or as a prefix, suffix, or prefix of another term, refers to a residue containing only carbon and hydrogen. This residue can be aliphatic or aromatic, linear, cyclic, bicyclic, branched, saturated, or unsaturated. It can also contain combinations of aliphatic, aromatic, linear, cyclic, bicyclic, branched, saturated, and unsaturated hydrocarbon moieties. However, when an alkyl group residue is described as substituted, it may optionally contain heteroatoms above and above the carbon and hydrogen members of the substituent residue. Thus, when specifically described as substituted, an alkyl group residue may also contain one or more carbonyl, amino, hydroxyl, etc., or it may contain heteroatoms within the backbone of the alkyl group residue. The term "alkyl" refers to a branched or linear, saturated aliphatic alkyl group, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, sec-pentyl, and n-hexyl and sec-hexyl. "Alkenyl" refers to a straight-chain or branched monovalent hydrocarbon group having at least one carbon-carbon double bond (e.g., vinyl (-HC=CH2)). "Alkoxy" refers to an alkyl group linked via oxygen (i.e., alkyl-O-), such as methoxy, ethoxy, and sec-butoxy. "Alkylene" refers to a straight-chain or branched, saturated, divalent aliphatic hydrocarbon group (e.g., methylene (-CH2-) or propylidene (-(CH2)3-)). "Cycloalkylene" refers to a divalent cyclic alkylene group, -C n H 2n-x The prefix "cycloalkenyl" refers to a monovalent group having one or more rings and one or more carbon-carbon double bonds within those rings, wherein all ring members are carbon (e.g., cyclopentyl and cyclohexyl). "Aryl" refers to an aromatic hydrocarbon group containing a specified number of carbon atoms, such as phenyl, cycloheptatrienone, indanyl, or naphthyl. "Arylene" refers to a divalent aryl group. "Alkyleneene" refers to an arylene substituted with an alkyl group. "Arylalkylene" refers to an alkylene substituted with an aryl group (e.g., benzyl). The prefix "halogenated" refers to a group or compound comprising one or more of fluorine, chlorine, bromine, or iodine substituents. Combinations of different halogen atoms (e.g., bromine and fluorine) or only chlorine atoms may be present. The prefix "heterogeneous" refers to a compound or group comprising at least one ring member containing heteroatoms (e.g., 1, 2, or 3 heteroatoms), wherein each heteroatom is independently N, O, S, Si, or P. "Substituted" means that a compound or group is substituted by at least one (e.g., 1, 2, 3, or 4) substituents, each of which can be C16 or C26 independently. 1-9 Alkoxy, C 1-9 Halogenated alkoxy, nitro (-NO2), cyano (-CN), C 1-6 alkylsulfonyl (-S(=O)2-alkyl), C 6-12 Arylsulfonyl (-S(=O)2-aryl), thiol (-SH), thiocyanate (-SCN), toluenesulfonyl (CH3C6H4SO2-), C3-12 cycloalkyl, C 2-12 alkenyl, C 5-12 Cycloalkenyl, C 6-12 Aryl, C 7-13 Arylalkylene, C 4-12 Heterocyclic alkyl groups, and C 3-12 A heteroaryl group can replace hydrogen, provided that the valence of the substituted atom does not exceed the normal valence of the substituted atom. The number of carbon atoms indicated in the group does not include any substituents. For example, -CH2CH2CN is a C2 alkyl group substituted with a nitrile.
[0156] While specific embodiments have been described, alternatives, modifications, variations, improvements, and substantial equivalents may be conceived by the applicant or others skilled in the art that are currently unforeseeable or likely to be unforeseeable. Therefore, the appended claims, as filed and as they may be modified, are intended to cover all such alternatives, modifications, variations, improvements, and substantial equivalents.
Claims
1. A composition comprising 53wt% to 68wt% of polyetherimide or poly(aryl ether sulfone); and 32wt% to 47wt% of filler; in, When the polymer is the polyetherimide, the filler comprises: Wollastonite fibers, with an average fiber diameter of 5 to 10 micrometers and an average fiber length of 55 to 75 micrometers, and a length of 2.5 m. 2 / g to less than 2.9m 2 / g surface area, 0.42g / cc to 0.50g / cc bulk density and 52% to 55% silica content; When the polymer is poly(aryl ether sulfone), the filler comprises: Wollastonite fibers, with an average fiber diameter of 1 to 5 micrometers and an average fiber length of 5 to 12 micrometers, 3.8m 2 / g to 4.3m 2 / g surface area and bulk density of 0.48g / cc to 0.56g / cc; or Boehmite, which has an average particle size (D50) of 0.4 μm to less than 0.9 μm as determined by laser scattering. Wherein, the weight percentage is based on the total weight of the composition, and The poly(arylene ether sulfone) is polyphenyl sulfone.
2. The composition according to claim 1, wherein the film formed from the composition exhibits: The coefficient of thermal expansion of flow is less than or equal to 36 ppm / °C, as determined by ASTM E831; and The percentage of transmission at 1330 nm greater than that measured by UV / Vis spectroscopy at a thickness of 100 μm.
3. The composition according to claim 1 or 2, comprising: 55 wt% to 65 wt% of the polyetherimide or the poly(aryl ether sulfone); and The filler is 35 wt% to 45 wt%.
4. The composition according to claim 1 or 2, comprising 58 wt% to 62 wt% of the polyetherimide or the poly(aryl ether sulfone); and The filler is 38 wt% to 42 wt%.
5. The composition according to claim 1 or 2, wherein the polyetherimide is present and the filler comprises the wollastonite, wherein the film formed from the composition exhibits: The coefficient of thermal expansion of the flow is less than or equal to 25 ppm / °C, as determined by ASTM D256; and The percentage of transmission at 1330 nm was greater than 50% at a thickness of 100 μm, determined by UV / Vis spectroscopy.
6. The composition according to claim 1 or 2, wherein the poly(aryl ether sulfone) is present and the filler comprises the wollastonite, wherein the film formed from the composition exhibits: The coefficient of thermal expansion of flow is less than or equal to 36 ppm / °C, as determined by ASTM E831; and The percentage of transmission at 1330 nm greater than that measured by UV / Vis spectroscopy at a thickness of 100 μm.
7. The composition according to claim 1 or 2, wherein the poly(aryl ether sulfone) is present and the filler comprises the boehmite, wherein the film formed from the composition exhibits: The coefficient of thermal expansion of the flow is less than or equal to 35 ppm / °C, as determined by ASTM E831; and The percentage of transmission at 1330 nm greater than that measured by UV / Vis spectroscopy at a thickness of 100 μm.
8. A method for preparing a composition according to any one of claims 1 to 7, the method comprising: The polyetherimide or the poly(aryl ether sulfone) is blended with the filler.
9. The method according to claim 8, wherein, The polyetherimide or the poly(aryl ether sulfone) is blended with the filler in the presence of a solvent.
10. The method according to claim 8 or 9, wherein, The polyetherimide or the poly(arylene ether sulfone) is blended with the filler at a temperature of 20°C to 200°C.
11. The method according to claim 8 or 9, wherein, The polyetherimide or the poly(arylene ether sulfone) is blended with the filler at a temperature of 20°C to 25°C or 175°C to 200°C.
12. A method of manufacturing a composition according to any one of claims 1 to 7, wherein the composition comprises the polyetherimide and the method comprises: Aromatic bis(ether anhydride) and organic amine are contacted to provide polyetherimide precursors; The filler is combined with the polyetherimide precursor to provide a mixture; and The mixture is heated under conditions that effectively provide the corresponding polyetherimide.
13. An article comprising the composition according to any one of claims 1 to 7.
14. The article of claim 13, wherein the article is an optical article.
15. The article of claim 13, wherein the article is an optical lens or lens array.
16. The article of claim 13, wherein the article is a transparent material used in medical devices, electronics and telecommunications, or buildings and structures.
17. The article of claim 13, wherein the article is a transparent material used in sensors, antennas, thin-film optics, or IR transparent display devices.
18. The article of claim 13, wherein the article is a transparent material used in an electrode, a thin film substrate, or a transistor.
Citation Information
Patent Citations
Production of aromatic polyethers
US4176222A
Cyclo-olefinic random copolymer, olefinic random copolymer, and process for producing cyclo-olefinic random copolymers
US5008356A
High temp. dimensionally stable reinforced polyolefin compsns. - comprising norbornene-ethylene! copolymer(s) and pref. glass fibres or asbestos
FR2407951A1
Composites transmissive to visual and infrared radiation and compositions and methods for making the composites
US20200140717A1