A preparation method and application of alumina ceramics

By forming core-shell powder in an alumina suspension and combining tartaric acid solution impregnation with external electric field sintering, the problem of uneven mixing of magnesium oxide and alumina was solved, and alumina ceramics with both high light transmittance and high mechanical strength were prepared, which are suitable for lighting fixtures.

CN116535196BActive Publication Date: 2024-11-12CHONGQING RES BETTER SCI & TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310582715.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-11-12
Estimated Expiration
2043-05-23

AI Technical Summary

Technical Problem

Existing technologies make it difficult to prepare transparent alumina ceramics that combine high light transmittance and high mechanical strength. Furthermore, the difficulty in uniformly mixing magnesium oxide and alumina leads to the formation of magnesium-rich regions, which hinders grain boundary movement and affects the densification of ceramic materials.

Method used

By adding soluble magnesium salts and ammonia to an alumina suspension to form a core-shell powder, and then impregnating it with tartaric acid solution and sintering it with an external electric field, combined with lithium chloride and aluminum chloride as sintering aids, the uniform densification and optical transmittance of alumina ceramics are promoted.

Benefits of technology

It achieves high light transmittance and high mechanical strength in alumina ceramics, making them suitable for lighting fixtures and improving the sintering density and optical transmittance of ceramic materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116535196B_ABST
    Figure CN116535196B_ABST
Patent Text Reader

Abstract

The invention relates to the field of ceramic materials, and in particular to a preparation method and application of an alumina ceramic. A soluble magnesium salt and ammonia water are added to an alumina suspension, and the mixture is heated in a water bath for reaction for 2-5 hours and then filtered to obtain a precursor. The precursor is calcined to obtain a core-shell powder. The core-shell powder is added to a tartaric acid solution for immersion, filtered out, dried, and then mixed with a sintering aid and ball-milled to obtain a mixed powder. The mixed powder is mixed and stirred evenly with an organic binder and injection-molded to obtain a green body. Under an external electric field, the green body is first heated and degreased and then sintered. The alumina ceramic prepared by the invention has both high light transmittance and high mechanical strength, and has broad application prospects in the field of lighting fixtures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of ceramic materials, and in particular to a preparation method and application of alumina ceramics. Background Art

[0002] Ceramics is a general term for pottery and porcelain, which can be divided into traditional ceramics and advanced ceramics, and transparent ceramics are a new type of advanced ceramic material developed in recent decades. Transparent ceramics refer to polycrystalline ceramic materials with a certain degree of light transmittance prepared by ceramic technology, also known as optical ceramics. Generally, ceramics with a linear transmittance of more than 10% are defined as transparent ceramics, and those with a linear transmittance of less than 10% are defined as translucent ceramics. Because traditional ceramics and conventional advanced ceramics have obvious scattering and absorption effects on visible light, they are usually opaque. In 1959, General Electric Company of the United States proposed that some ceramics have light transmittance. In 1962, Coble and others of the company prepared translucent alumina ceramics for the first time, opening up a new research direction in the field of advanced ceramic materials. With the advancement of science and technology, transparent alumina ceramics have become an important part of advanced ceramic materials. How to prepare transparent alumina ceramics with both high light transmittance and high mechanical strength has become the current research focus. Summary of the invention

[0003] Purpose of the invention: In view of the above technical problems, the present invention proposes a preparation method and application of alumina ceramics.

[0004] The technical solutions adopted are as follows:

[0005] A method for preparing alumina ceramics is as follows:

[0006] S1: preparing alumina suspension;

[0007] S2: adding soluble magnesium salt and ammonia water to the alumina suspension, heating in a water bath for 2-5 hours and then filtering to obtain a precursor;

[0008] S3: calcining the precursor to obtain core-shell powder;

[0009] S4: adding the core-shell powder into a tartaric acid solution for immersion, filtering out, drying, and then mixing with a sintering aid and ball milling to obtain a mixed powder; mixing the mixed powder with an organic binder and stirring evenly, and injection molding to obtain a green body; and heating and degreasing the green body under an external electric field and then sintering it.

[0010] Furthermore, the preparation method of the alumina suspension in S1 is as follows:

[0011] Alumina powder, dispersant and water are mixed, stirred evenly and ultrasonically vibrated for 10-30 minutes to obtain a suspension with a solid content of 3-6%.

[0012] Furthermore, the dispersant is polyacrylic acid and triammonium citrate, and the mass ratio of the polyacrylic acid to triammonium citrate is 1-5:1.

[0013] Furthermore, in S3, the calcination temperature is 600-800° C., and the calcination time is 2-4 hours.

[0014] Furthermore, the sintering aid in S4 is a metal chloride.

[0015] Furthermore, the metal chloride is a combination of lithium chloride and aluminum chloride, and the mass ratio of the lithium chloride to the aluminum chloride is 1-5:1-5.

[0016] Furthermore, the amount of the sintering aid in S4 is 0.05-0.1% of the mass of the core-shell powder.

[0017] Furthermore, the organic binder in S4 includes polyvinyl butyral, microcrystalline wax, stearic acid and plasticizer, and the mass ratio of polyvinyl butyral, microcrystalline wax, stearic acid and plasticizer is 10-15:3-5:3-5:1.

[0018] Furthermore, the temperature of heating and debinding in S4 is 500-600°C, the time is 2-6h, and the sintering temperature is 1650-1800°C, the time is 2-4h.

[0019] The present invention also provides an application of the alumina ceramics prepared by the above method in lighting fixtures.

[0020] Beneficial effects of the present invention:

[0021] The present invention provides a method for preparing an alumina ceramic. Magnesium oxide is a commonly used additive for alumina ceramics. After being added, it can improve the sintering density of the alumina ceramics, and enhance the mechanical strength and optical transmittance. However, if magnesium oxide is directly added, it is difficult to completely mix the alumina and magnesium oxide, and a magnesium-rich region will inevitably be formed. Since magnesium oxide has a lower density and worse sintering performance, excessive magnesium oxide in the magnesium-rich region hinders the movement of grain boundaries, which is not conducive to the densification of ceramic materials. The inventor uses homogeneous precipitation to uniformly coat magnesium oxide on the surface of alumina powder so that the two are in full contact, thereby avoiding the formation of magnesium-rich regions and improving the sintering density and optical transmittance.

[0022] The optical transmittance of alumina ceramics can be greatly improved by impregnating core-shell powder with tartaric acid. The reason may be that tartaric acid complexes with impurity elements in the core-shell powder to remove them, and reacts with magnesium oxide to form magnesium tartrate, which promotes the nucleation of alumina, thereby reducing the sintering temperature and promoting the improvement of ceramic density.

[0023] The sintering aids composed of lithium chloride and aluminum chloride can inhibit the growth of grains, shorten the diffusion distance of pores in the crystal, and further accelerate the sintering process to improve the density;

[0024] Sintering under an applied electric field can more easily form cubic alumina without optical anisotropy, and can also reduce the generation of pores and improve density and optical transmittance.

[0025] The alumina ceramics prepared by the present invention have both high light transmittance and high mechanical strength, and have broad application prospects in the field of lighting fixtures. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a physical picture of the alumina ceramic prepared in Example 1 of the present invention;

[0027] Figure 2 This is a comparison chart of the linear transmittance of alumina ceramics prepared in Example 1 of the present invention and Comparative Examples 1-4. DETAILED DESCRIPTION

[0028] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.

[0029] Embodiment 1:

[0030] A method for preparing alumina ceramics:

[0031] Take 100g of α-alumina powder with a purity of 99.99%, 0.5g of polyacrylic acid, 0.1g of triammonium citrate, and 3L of water, mix them, stir them evenly, and then ultrasonically oscillate them for 20 minutes to obtain an alumina suspension with a solid content of 3.2%. Add 7.4g of magnesium nitrate to the alumina suspension, adjust the pH of the system to 9.5 with 30% ammonia water, heat in a water bath at 80°C for 4h, and then filter to obtain a precursor. Transfer the precursor to an oven and dry it at 80°C for 24h. Heat the precursor to 600°C at a rate of 10°C / min and calcine it for 3h to obtain a core-shell powder. Add the above core-shell powder to 500mL Stir and immerse in 10wt% tartaric acid solution at room temperature for 2h, then filter out, dry at 80℃ for 24h, take 100g and mix with 0.05g lithium chloride and 0.05g aluminum chloride and ball mill for 2h to get mixed powder, mix 15g polyvinyl butyral, 5g microcrystalline wax, 5g stearic acid and 1g plasticizer DOP at 140℃ for 0.5h to become a uniform colloidal liquid, then gradually add the mixed powder while stirring, and continue to stir at high speed for 1h until the feeding is uniform. , and then granulate to obtain granular feed, put the granular feed into an injection machine for injection molding to obtain a green body, the injection pressure is 20MPa, the injection temperature is 90℃, the mold is directly connected to the ice water cooling system, the cooling water temperature is 0℃, the green body is placed in a hot stripping furnace and heated to 600℃ at a rate of 10℃ / min under an external electric field strength of 200kV / cm, degreased for 6h, then heated to 1780℃ at a rate of 5℃ / min, sintered for 2h, and cooled to room temperature with the furnace.

[0032] The prepared alumina ceramics were used as samples to test the light transmittance. The thickness of the samples was 1 mm. The linear transmittance test was performed using an ultraviolet-visible spectrometer (UV-1800, Mapada, Shanghai) with a wavelength range of 300-1100 nm. The results are shown in Figure 2. Figure 1 shown.

[0033] The flexural strength of the sample was measured by the three-point bending method (AGS-X-20KN, Shimadzu, Japan) and was 583 MPa.

[0034] Embodiment 2:

[0035] A method for preparing alumina ceramics:

[0036] Take 100g of α-alumina powder with a purity of 99.99%, 0.5g of polyacrylic acid, 0.1g of triammonium citrate, and 3L of water, mix them, stir them evenly, and then ultrasonically oscillate for 30min to obtain an alumina suspension with a solid content of 3.2%, add 7.4g of magnesium nitrate to the alumina suspension, adjust the pH of the system to 9.5 with 30% ammonia water, heat in a water bath at 80°C for 4h, and then filter to obtain a precursor, transfer the precursor to an oven and dry it at 80°C for 24h, heat the precursor to 800°C at a rate of 10°C / min and calcine it for 4h to obtain a core-shell powder, and add the above core-shell powder to 500mL Stir and immerse in 10wt% tartaric acid solution at room temperature for 2h, then filter out, dry at 80℃ for 24h, take 100g and mix with 0.05g lithium chloride and 0.05g aluminum chloride and ball mill for 2h to get mixed powder, mix 15g polyvinyl butyral, 5g microcrystalline wax, 5g stearic acid and 1g plasticizer DOP at 140℃ for 0.5h to become a uniform colloidal liquid, then gradually add the mixed powder while stirring, and continue to stir at high speed for 1h until the feeding is uniform. , and then granulate to obtain granular feed, put the granular feed into an injection machine for injection molding to obtain a green body, the injection pressure is 20MPa, the injection temperature is 90℃, the mold is directly connected to the ice water cooling system, the cooling water temperature is 0℃, the green body is placed in a hot stripping furnace and heated to 600℃ at a rate of 10℃ / min under an external electric field strength of 200kV / cm, degreased for 6h, then heated to 1800℃ at a rate of 5℃ / min, sintered for 4h, and cooled to room temperature with the furnace.

[0037] The flexural strength of the sample was measured by the three-point bending method (AGS-X-20KN, Shimadzu, Japan) and was 570 MPa.

[0038] Embodiment 3:

[0039] A method for preparing alumina ceramics:

[0040] Take 100g of α-alumina powder with a purity of 99.99%, 0.5g of polyacrylic acid, 0.1g of triammonium citrate, and 3L of water, mix them, stir them evenly, and then ultrasonically oscillate for 10min to obtain an alumina suspension with a solid content of 3.2%, add 7.4g of magnesium nitrate to the alumina suspension, adjust the pH of the system to 9.5 with 30% ammonia water, heat in a water bath at 80°C for 4h, and then filter to obtain a precursor, transfer the precursor to an oven and dry it at 80°C for 24h, heat the precursor to 600°C at a rate of 10°C / min and calcine it for 2h to obtain a core-shell powder, and add the above core-shell powder to 500mL Stir and immerse in 10wt% tartaric acid solution at room temperature for 2h, then filter out, dry at 80℃ for 24h, take 100g and mix with 0.05g lithium chloride and 0.05g aluminum chloride and ball mill for 2h to get mixed powder, mix 10g polyvinyl butyral, 3g microcrystalline wax, 3g stearic acid and 1g plasticizer DOP at 140℃ for 0.5h to become a uniform colloidal liquid, then gradually add the mixed powder while stirring, and continue to stir at high speed for 1h until the feeding is uniform. , and then granulate to obtain granular feed, put the granular feed into an injection machine for injection molding to obtain a green body, the injection pressure is 20MPa, the injection temperature is 90℃, the mold is directly connected to the ice water cooling system, the cooling water temperature is 0℃, the green body is placed in a hot stripping furnace and heated to 500℃ at a rate of 10℃ / min under an external electric field strength of 200kV / cm for degreasing for 6h, then heated to 1700℃ at a rate of 5℃ / min for sintering for 2h, and then cooled to room temperature with the furnace.

[0041] The flexural strength of the sample was measured by the three-point bending method (AGS-X-20KN, Shimadzu, Japan) and was 556 MPa.

[0042] Embodiment 4:

[0043] A method for preparing alumina ceramics:

[0044] Take 100g of α-alumina powder with a purity of 99.99%, 0.5g of polyacrylic acid, 0.1g of triammonium citrate, and 3L of water, mix them, stir them evenly, and then ultrasonically oscillate for 30min to obtain an alumina suspension with a solid content of 3.2%, add 7.4g of magnesium nitrate to the alumina suspension, adjust the pH of the system to 9.5 with 30% ammonia water, heat in a water bath at 80°C for 4h, and then filter to obtain a precursor, transfer the precursor to an oven and dry it at 80°C for 24h, heat the precursor to 600°C at a rate of 10°C / min and calcine it for 4h to obtain a core-shell powder, and add the above core-shell powder to 500mL Stir and immerse in 10wt% tartaric acid solution at room temperature for 2h, then filter out, dry at 80℃ for 24h, take 100g and mix with 0.05g lithium chloride and 0.05g aluminum chloride and ball mill for 2h to get mixed powder, mix 10g polyvinyl butyral, 5g microcrystalline wax, 3g stearic acid and 1g plasticizer DOP at 140℃ for 0.5h to form a uniform colloidal liquid, then gradually add the mixed powder while stirring, and continue to stir at high speed for 1h until the feeding is uniform. , and then granulate to obtain granular feed, put the granular feed into an injection machine for injection molding to obtain a green body, the injection pressure is 20MPa, the injection temperature is 90℃, the mold is directly connected to the ice water cooling system, the cooling water temperature is 0℃, the green body is placed in a hot stripping furnace and heated to 600℃ at a rate of 10℃ / min under an external electric field strength of 200kV / cm for degreasing for 6h, then heated to 1800℃ at a rate of 5℃ / min for sintering for 2h, and then cooled to room temperature with the furnace.

[0045] The flexural strength of the sample was measured by the three-point bending method (AGS-X-20KN, Shimadzu, Japan) and was 572 MPa.

[0046] Embodiment 5:

[0047] A method for preparing alumina ceramics:

[0048] Take 100g of α-alumina powder with a purity of 99.99%, 0.5g of polyacrylic acid, 0.1g of triammonium citrate, and 3L of water, mix them, stir them evenly, and then ultrasonically oscillate for 10 minutes to obtain an alumina suspension with a solid content of 3.2%. Add 7.4g of magnesium nitrate to the alumina suspension, adjust the pH of the system to 9.5 with 30% ammonia water, heat in a water bath at 80°C for 4h, and then filter to obtain a precursor. Transfer the precursor to an oven and dry it at 80°C for 24h. Heat the precursor to 800°C at a rate of 10°C / min and calcine it for 2h to obtain a core-shell powder. Add the above core-shell powder to 500mL Stir and immerse in 10wt% tartaric acid solution at room temperature for 2h, then filter out, dry at 80℃ for 24h, take 100g and mix with 0.05g lithium chloride and 0.05g aluminum chloride and ball mill for 2h to get mixed powder, mix 15g polyvinyl butyral, 3g microcrystalline wax, 5g stearic acid and 1g plasticizer DOP at 140℃ for 0.5h to form a uniform colloidal liquid, then gradually add the mixed powder while stirring, and continue to stir at high speed for 1h until the feeding is uniform. , and then granulate to obtain granular feed, put the granular feed into an injection machine for injection molding to obtain a green body, the injection pressure is 20MPa, the injection temperature is 90℃, the mold is directly connected to the ice water cooling system, the cooling water temperature is 0℃, the green body is placed in a hot stripping furnace and heated to 500℃ at a rate of 10℃ / min under an external electric field strength of 200kV / cm for degreasing for 6h, then heated to 1750℃ at a rate of 5℃ / min for sintering for 3h, and then cooled to room temperature with the furnace.

[0049] The flexural strength of the sample was measured by the three-point bending method (AGS-X-20KN, Shimadzu, Japan) and was 561 MPa.

[0050] Comparative Example 1:

[0051] The method is basically the same as Example 1, except that the same mass of magnesium oxide is directly added for ball milling without coating.

[0052] The prepared alumina ceramics were used as samples to test the light transmittance. The thickness of the samples was 1 mm. The linear transmittance test was performed using an ultraviolet-visible spectrometer (UV-1800, Mapada, Shanghai) with a wavelength range of 300-1000 nm. The results are shown in Figure 2. Figure 1 shown.

[0053] The flexural strength of the sample was measured by the three-point bending method (AGS-X-20KN, Shimadzu, Japan) and was 569 MPa.

[0054] Comparative Example 2:

[0055] The method is substantially the same as Example 1, except that tartaric acid impregnation is not performed.

[0056] The prepared alumina ceramics were used as samples to test the light transmittance. The thickness of the samples was 1 mm. The linear transmittance test was performed using an ultraviolet-visible spectrometer (UV-1800, Mapada, Shanghai) with a wavelength range of 300-1000 nm. The results are shown in Figure 2. Figure 1 shown.

[0057] The flexural strength of the sample was measured by the three-point bending method (AGS-X-20KN, Shimadzu, Japan) and was 574 MPa.

[0058] Comparative Example 3:

[0059] The method is substantially the same as Example 1, except that lithium chloride is replaced by aluminum chloride.

[0060] The prepared alumina ceramics were used as samples to test the light transmittance. The thickness of the samples was 1 mm. The linear transmittance test was performed using an ultraviolet-visible spectrometer (UV-1800, Mapada, Shanghai) with a wavelength range of 300-1000 nm. The results are shown in Figure 2. Figure 1 shown.

[0061] The flexural strength of the sample was measured by the three-point bending method (AGS-X-20KN, Shimadzu, Japan) and was 532 MPa.

[0062] Comparative Example 4:

[0063] It is basically the same as Example 1, except that the external electric field is removed.

[0064] The prepared alumina ceramics were used as samples to test the light transmittance. The thickness of the samples was 1 mm. The linear transmittance test was performed using an ultraviolet-visible spectrometer (UV-1800, Mapada, Shanghai) with a wavelength range of 300-1000 nm. The results are shown in Figure 2. Figure 1 shown.

[0065] The flexural strength of the sample was measured by the three-point bending method (AGS-X-20KN, Shimadzu, Japan) and was 580 MPa.

[0066] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing an alumina ceramic, characterized in that: The details are as follows: S1: preparing alumina suspension; S2: adding soluble magnesium salt and ammonia water to the alumina suspension, heating in a water bath for 2-5 hours and then filtering to obtain a precursor; S3: calcining the precursor to obtain core-shell powder; In S3, the calcination temperature is 600-800°C and the calcination time is 2-4h; S4: adding the core-shell powder into a tartaric acid solution for immersion, filtering out, drying, and then mixing with a sintering aid and ball milling to obtain a mixed powder, mixing the mixed powder with an organic binder and stirring evenly, and injection molding to obtain a green body, and heating and degreasing the green body under an external electric field and then sintering it; The sintering aid in S4 is a metal chloride; The metal chloride is a combination of lithium chloride and aluminum chloride, and the mass ratio of lithium chloride to aluminum chloride is 1-5:1-5; The amount of the sintering aid in S4 is 0.05-0.1% of the mass of the core-shell powder.

2. The method for preparing alumina ceramics according to claim 1, characterized in that: The preparation method of the alumina suspension described in S1 is as follows: Alumina powder, dispersant and water are mixed, stirred evenly and ultrasonically vibrated for 10-30 minutes to obtain a suspension with a solid content of 3-6%.

3. The method for preparing alumina ceramics according to claim 2, characterized in that: The dispersant is polyacrylic acid and triammonium citrate, and the mass ratio of the polyacrylic acid to triammonium citrate is 1-5:

1.

4. The method for preparing alumina ceramics according to claim 1, characterized in that: The organic binder in S4 includes polyvinyl butyral, microcrystalline wax, stearic acid and plasticizer, and the mass ratio of polyvinyl butyral, microcrystalline wax, stearic acid and plasticizer is 10-15:3-5:3-5:

1.

5. The method for preparing alumina ceramics according to claim 1, characterized in that: The heating and debinding temperature in S4 is 500-600°C, the time is 2-6h, and the sintering temperature is 1650-1800°C, the time is 2-4h.

6. Use of alumina ceramics prepared by the method for preparing alumina ceramics as described in any one of claims 1 to 5 in lighting fixtures.

Citation Information

Patent Citations

  • Preparation method for nanocrystalline alumina ceramic

    CN105948726A

  • Preparation method of fluorescent ceramic containing aluminum oxide matrix and related fluorescent ceramic

    CN107285746A

  • Preparation method of high-strength semitransparent aluminum oxide ceramic

    CN111153688A

  • Submicron spherical aluminum oxide as well as preparation method and application thereof

    CN111392752A

  • Zirconia-Alumina nano-composite powder and preparationmethod thereof

    KR1020060052129A