Preparation method of low-temperature solid-phase sintered self-synthesized MgAl2O4 ceramic

Through the low-temperature solid phase sintering self-synthesis method, MgAl2O4 ceramics are generated by reaction of activated alumina and TiO2, which solves the problems of high sintering temperature and poor density, and realizes the preparation of high thermal conductivity and high strength ceramic materials, reducing production costs.

CN118930244APending Publication Date: 2024-11-12HUNAN UNIV OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410908165.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing MgAl2O4 ceramics have high sintering temperature, which leads to high sintering cost and poor material density, especially the sintering performance of samples rich in alumina.

Method used

The low-temperature solid phase sintering self-synthesis method is adopted. By mixing aluminum oxide, magnesium oxide and titanium dioxide powder, reacting with alkaline solution and organic matter to form a gel liquid. After dehydration and degreasing treatment, it is finally sintered at 1480-1550℃. The active Al2O3 and TiO2 react to form dense MgAl2O4 ceramics.

Benefits of technology

The sintering temperature is reduced, the density and thermal conductivity of the material are improved, the production cost is reduced, and the strength and bending strength of the material are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930244A_ABST
    Figure CN118930244A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of self-synthesized MgAl2O4 ceramic by low-temperature solid-phase sintering, which comprises the following steps: homogenizing active Al2O3, MgO and TiO2, performing gel forming, dehydrating and degreasing, and finally performing high-temperature sintering to obtain the MgAl2O4 ceramic. According to the invention, active Al2O3 and MgO are subjected to reaction sintering to generate compact MgAl2O4 ceramic, the active alumina has high activity, good sinterability and reaction capability, TiO2 is used as a sintering aid, the vacancy concentration of MgAl2O4 crystals is improved, the MgAl2O4 structure is distorted, crystal lattices are activated, the diffusion sintering of the material is promoted, and the sintering density of the material is improved. According to the invention, the gel-state liquid is adopted to realize high-uniformity distribution and blank forming of the mixed powder, and the MgAl2O4 ceramic with high density can be obtained by sintering at the highest temperature of 1550 DEG C, so that the problem of high sintering temperature of the existing MgAl2O4 ceramic is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of MgAl2O4 ceramics, and more specifically, relates to a preparation method of low-temperature solid-phase sintering self-synthesized MgAl2O4 ceramics. Background Art

[0002] MgAl2O4 ceramic materials have excellent thermal, mechanical, optical, dielectric and chemical properties, and are widely used in refractory materials, optical transparent windows, pigments, phosphors and inert matrix fuels. MgAl2O4 has a large negative Gibbs free energy, excellent thermal shock and corrosion resistance, and stable physical and chemical properties at high temperatures, which makes it have a promising application prospect in high-temperature industries; the addition of transition metal ions to MgAl2O4 single crystals can refine and split the energy levels of the crystals, showing unique spectral characteristics, and can be applied to acoustic and microwave devices; MgAl2O4 single crystals have good insulation properties such as low dielectric constant and loss, and good matching with Si and other important oxide system lattice structures. It is a fast IC epitaxial substrate material. At the same time, studies have found that it can also be used as a substrate material for III-V nitride devices due to its energy level characteristics; its low acidity and good thermal stability make MgAl2O4 an excellent catalyst for the oxidation of sulfur dioxide to sulfur dioxide, and it has applications in the fields of environment, petroleum processing and fine chemical production.

[0003] When the prior art uses the influence of the content of alumina raw materials on the densification behavior of MgAl2O4 during high-temperature sintering, it is found that compared with MgAl2O4 rich in magnesium oxide, MgAl2O4 rich in alumina exhibits poor sintering performance. This is because the sample rich in alumina exhibits larger grains, which affects the compactness. In the sample rich in magnesium oxide, there are second-phase magnesium oxide particles at the grain boundaries, which limits the migration of the grain boundaries, making the generated MgAl2O4 grains dense and small. CN202310664307.0 A high-purity and high-density sintered magnesium aluminum spinel and its preparation method discloses that after a high-purity industrial alumina filter material and a high-purity basic magnesium carbonate filter material are evenly mixed, they are calcined at high temperature to obtain a high-purity magnesium aluminum spinel light-burned powder; the high-purity magnesium aluminum spinel light-burned powder is pressed and calcined at ultra-high temperature in turn to obtain a ceramic high-performance refractory material. The patent uses a low-temperature and high-pressure carbonization method to pre-treat industrial alumina and light-burned magnesium oxide to obtain high-purity alumina basic magnesium carbonate. The high-purity magnesium aluminum spinel light-burned powder synthesized by pre-sintering has good sintering activity and sufficient spinel content (≥50%), which can offset the expansion effect caused by the generation of spinel during ultra-high temperature sintering, thereby improving the density in the subsequent high-temperature sintering. However, the sintering temperature used is as high as 1800-1900℃, which undoubtedly greatly increases the sintering cost. Even though the volume density and physical properties of MgAl2O4 can be effectively improved by doping some sintering aids, Ma Beiyue et al. (L. Yuan, B. Ma, Q. Zhu, Z. Wang, G. Li, J. Yu. Preparation and properties of MgAl2O4 based ceramics reinforced with rod-like microcrystallines by co-doping Sm2O3 and La2O3 [J]. Ceramics International, 2017, 43 (18): 16258-16263.) successfully prepared dense MgAl2O4 based ceramics by composite addition of Sm2O3 and La2O3 and a one-step reaction sintering process at 1680 ° C for 4 h. The additives generate rod-shaped Sm4.67(SiO4)3O and La4.67(SiO4)3O microcrystalline compounds in the MgAl2O4 matrix. These compounds prevent the growth of MgAl2O4 grains, effectively remove impurities in the grain boundaries, and improve the compressive strength and thermal shock resistance of ceramic materials. However, most of the research sintering temperatures are above 1600℃, which places high demands on sintering equipment and makes the research cost high. Summary of the invention

[0004] In order to overcome the problem of high sintering temperature of existing MgAl2O4 ceramics, the invention provides a preparation method of low-temperature solid-phase sintering self-synthesized MgAl2O4 ceramics.

[0005] The present invention is achieved through the following technical solutions:

[0006] A method for preparing low-temperature solid-phase sintering self-synthesized MgAl2O4 ceramics, the preparation steps comprising:

[0007] S1. The aluminum oxide, magnesium oxide and titanium dioxide powders are mixed uniformly to obtain a mixed powder;

[0008] S2. The mixed powder is mixed with an alkaline solution, aged, and then an organic matter is added to form a gel-like liquid and cross-linked to form a body;

[0009] S3. The green body is dehydrated at 50-100 ° C, and then heated to 1000 ° C for degreasing;

[0010] S4. The degreased green body is heated to 1480-1550° C. for sintering, and the MgAl 2 O 4 ceramic material is obtained after cooling.

[0011] Furthermore, the mass ratio of aluminum oxide to magnesium oxide is 70-75:25-30.

[0012] Furthermore, the addition amount of titanium dioxide is 1-4% of the total mass of aluminum oxide and magnesium oxide.

[0013] Furthermore, the mass ratio of the mixed powder to the organic matter is 2 to 4:1.

[0014] Furthermore, the mixed powder is pre-treated by ball milling, the mass ratio of the mixed powder, ball mill stone and alcohol is 1:1:2, the rotation speed of the ball mill is 200-300 r / min, and the ball milling is performed for 5-8 hours.

[0015] Furthermore, the organic matter includes a monomer, a cross-linking agent, an initiator and a catalyst, and the mass ratio thereof is 8:2:1:1.

[0016] Furthermore, the monomer is one or more of acrylic acid, dimethylacrylamide, dimethylaminomethacrylate, methacrylate, and hydroxyethyl acrylate; the crosslinking agent is one or more of N,N-methyleneacrylamide and isocyanate; the initiator includes one or more of persulfates, tert-butyl hydroperoxide, sodium pyrosulfite, and sucrose; the catalyst is one or more of tetramethylethylenediamine, Lewis acid, and polyacrylamide.

[0017] Furthermore, the heating stage of the heating degreasing includes: heating from 100°C to 200-400°C, keeping warm for 2-3 hours, then heating to 420-800°C, keeping warm for 2-3 hours, and finally heating to 1000°C and keeping warm to complete the degreasing.

[0018] Furthermore, the heating rate of the degreasing process is 3-6°C / min.

[0019] Furthermore, the heating rate of the sintering is 3-6°C / min, and the sintering holding time is 2-3h.

[0020] Compared with the prior art, the beneficial effects are:

[0021] The present invention uses active Al2O3 and MgO to react and sinter to generate dense MgAl2O4 ceramics, uses active alumina with high activity, good sinterability and reactivity, and uses TiO2 as a sintering aid to increase the vacancy concentration of the MgAl2O4 crystal, distort the MgAl2O4 structure, activate the lattice, thereby promoting the diffusion sintering of the material and improving the sintering density of the material. The present invention uses a gel-state liquid to achieve high uniform distribution and green body forming of the mixed powder, and sintering at a maximum temperature of 1550°C can obtain a high-density MgAl2O4 ceramic, effectively improving the thermal conductivity and strength of the material, reducing the sintering temperature and thus reducing the production cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 XRD diffraction patterns of different TiO2 contents sintered at 1550℃;

[0023] Figure 2 SEM images of different TiO2 contents at 1550℃;

[0024] Figure 3 SEM images of 3%wtTiO2 samples at different sintering temperatures DETAILED DESCRIPTION

[0025] The following is further explained and illustrated in conjunction with the examples, but the specific examples do not limit the present invention in any form. If not specifically stated, the methods and equipment used in the examples are conventional methods and equipment in the art, and the raw materials used are all conventional commercially available raw materials.

[0026] Example 1

[0027] This embodiment provides a method for preparing low-temperature solid-phase sintering self-synthesized MgAl2O4 ceramics, the steps comprising:

[0028] S1. Use anhydrous ethanol as dispersant and Al2O3 balls as grinding media. Mix Al2O3 and MgO powders in a mass ratio of 71.8:28.2, add 1% TiO2 of the powder mass, put them into a corundum ball mill, rotate at 280r / min, run for 6h, and mix the raw materials thoroughly.

[0029] S2. Pour the ball-milled mixture into an evaporating dish, and place the evaporating dish in a constant temperature oven for drying. The oven temperature is set at 50°C. After it is completely dried, take out the raw material, gently scrape it into the sieve with a medicine spoon, and continue to grind until the raw material completely passes through the 80-mesh sieve to form a mixed powder.

[0030] S3. Add organic monomers acrylic acid (AA), N,N-dimethylacrylamide (DMAA), crosslinking agent N,N-methyleneacrylamide (MBAM), dispersant PEG400, PEG1000, and ammonium polyacrylate (NH4PAA) to the mixed powder, add them into water for full dissolution and mixing, so that the powder forms a gel liquid, and add initiators potassium persulfate and sodium persulfate, and catalyst tetramethylethylenediamine to the gel liquid. Finally, inject and solidify into sheets to obtain a green body with high strength and a bending strength of 20-40MPa.

[0031] S4. Dehydrate the green body at 50-100℃ to slowly remove the water in the green body. Then, heat the green body from 100℃ to 1000℃ at 5℃ / min, and keep the temperature at 400℃ and 800℃ for 2h respectively to ensure complete degreasing.

[0032] S5. Finally, the temperature was raised from 1000°C to 1550°C at a rate of 5°C / min and kept at that temperature for 3 hours, and then cooled to room temperature in the furnace to obtain MgAl2O4 ceramics.

[0033] Example 2

[0034] This embodiment provides a method for preparing low-temperature solid-phase sintering self-synthesized MgAl2O4 ceramics, the steps comprising:

[0035] S1. Use anhydrous ethanol as dispersant and Al2O3 balls as grinding media. Mix Al2O3 and MgO powders in a mass ratio of 71.8:28.2, add 2% TiO2 based on the mass of the powder, put them into a corundum ball mill, rotate at 280r / min, run for 6h, and mix the raw materials thoroughly.

[0036] S2. Pour the ball-milled mixture into an evaporating dish, and place the evaporating dish in a constant temperature oven for drying. The oven temperature is set at 50°C. After it is completely dried, take out the raw material, gently scrape it into the sieve with a medicine spoon, and continue to grind until the raw material completely passes through the 80-mesh sieve to form a mixed powder.

[0037] S3. Mechanically mix the mixed powder with the alkaline solution, then age it, add the organic monomers acrylic acid (AA), N,N-dimethylacrylamide (DMAA), crosslinker N,N-methyleneacrylamide (MBAM), dispersant PEG400, PEG1000, and ammonium polyacrylate (NH4PAA) into water for full dissolution and mixing, so that the powder forms a gel liquid, and add initiators potassium persulfate and sodium persulfate, and catalyst tetramethylethylenediamine into the gel liquid. Finally, inject and solidify it into a sheet to obtain a green body with high strength and a bending strength of 20-40MPa.

[0038] S4. Dehydrate the green body at 50-100℃ to slowly remove the water in the green body. Then, heat the green body from 100℃ to 1000℃ at 5℃ / min, and keep the temperature at 400℃ and 800℃ for 2h respectively to ensure complete degreasing.

[0039] S5. Finally, the temperature was raised from 1000°C to 1550°C at a rate of 5°C / min and kept at that temperature for 3 hours, and then cooled to room temperature in the furnace to obtain MgAl2O4 ceramics.

[0040] Example 3

[0041] This embodiment provides a method for preparing low-temperature solid-phase sintering self-synthesized MgAl2O4 ceramics, the steps comprising:

[0042] S1. Use anhydrous ethanol as dispersant and Al2O3 balls as grinding media. Mix Al2O3 and MgO powders in a mass ratio of 71.8:28.2, add 3% TiO2 based on the mass of the powder, put them into a corundum ball mill, rotate at 280r / min, run for 6h, and mix the raw materials thoroughly.

[0043] S2. Pour the ball-milled mixture into an evaporating dish, and place the evaporating dish in a constant temperature oven for drying. The oven temperature is set at 50°C. After it is completely dried, take out the raw material, gently scrape it into the sieve with a medicine spoon, and continue to grind until the raw material completely passes through the 80-mesh sieve to form a mixed powder.

[0044] S3. Mechanically mix the mixed powder with the alkaline solution, then age it, add the organic monomers acrylic acid (AA), N,N-dimethylacrylamide (DMAA), crosslinker N,N-methyleneacrylamide (MBAM), dispersant PEG400, PEG1000, and ammonium polyacrylate (NH4PAA) into water for full dissolution and mixing, so that the powder forms a gel liquid, and add initiators potassium persulfate and sodium persulfate, and catalyst tetramethylethylenediamine into the gel liquid. Finally, inject and solidify it into a sheet to obtain a green body with high strength and a bending strength of 20-40MPa.

[0045] S4. Dehydrate the green body at 50-100℃ to slowly remove the water in the green body. Then, heat the green body from 100℃ to 1000℃ at 5℃ / min, and keep the temperature at 400℃ and 800℃ for 2h respectively to ensure complete degreasing.

[0046] S5. Finally, the temperature was raised from 1000°C to 1550°C at a rate of 5°C / min and kept at that temperature for 3 hours, and then cooled to room temperature in the furnace to obtain MgAl2O4 ceramics.

[0047] Example 4

[0048] This embodiment provides a method for preparing low-temperature solid-phase sintering self-synthesized MgAl2O4 ceramics, the steps comprising:

[0049] S1. Use anhydrous ethanol as dispersant and Al2O3 balls as grinding media. Mix Al2O3 and MgO powders in a mass ratio of 71.8:28.2, add 4% TiO2 of the powder mass, put them into a corundum ball mill, rotate at 280r / min, run for 6h, and mix the raw materials thoroughly.

[0050] S2. Pour the ball-milled mixture into an evaporating dish, and place the evaporating dish in a constant temperature oven for drying. The oven temperature is set at 50°C. After it is completely dried, take out the raw material, gently scrape it into the sieve with a medicine spoon, and continue to grind until the raw material completely passes through the 80-mesh sieve to form a mixed powder.

[0051] S3. Mechanically mix the mixed powder with the alkaline solution, then age it, add the organic monomers acrylic acid (AA), N,N-dimethylacrylamide (DMAA), crosslinker N,N-methyleneacrylamide (MBAM), dispersant PEG400, PEG1000, and ammonium polyacrylate (NH4PAA) into water for full dissolution and mixing, so that the powder forms a gel liquid, and add initiators potassium persulfate and sodium persulfate, and catalyst tetramethylethylenediamine into the gel liquid. Finally, inject and solidify it into a sheet to obtain a green body with high strength and a bending strength of 20-40MPa.

[0052] S4. Dehydrate the green body at 50-100℃ to slowly remove the water in the green body. Then, heat the green body from 100℃ to 1000℃ at 5℃ / min, and keep the temperature at 400℃ and 800℃ for 2h respectively to ensure complete degreasing.

[0053] S5. Finally, the temperature was raised from 1000°C to 1550°C at a rate of 5°C / min and kept at that temperature for 3 hours, and then cooled to room temperature in the furnace to obtain MgAl2O4 ceramics.

[0054] Example 5

[0055] The present embodiment provides a method for preparing a low-temperature solid-phase sintered self-synthesized MgAl2O4 ceramic, and its process is the same as that of Example 2, except that in this embodiment, the temperature is finally raised from 1000°C to 1500°C at 5°C / min in S5 and kept at this temperature for 3 hours, and then cooled to room temperature with the furnace to obtain a high thermal conductivity and high strength MgAl2O4 ceramic.

[0056] Example 6

[0057] The present embodiment provides a method for preparing a low-temperature solid-phase sintered self-synthesized MgAl2O4 ceramic, and its process is the same as that of Example 3, except that in this embodiment, the temperature is finally raised from 1000°C to 1500°C at 5°C / min in S5 and kept at this temperature for 3 hours, and then cooled to room temperature in the furnace to obtain a high thermal conductivity and high strength MgAl2O4 ceramic.

[0058] Example 7

[0059] The present embodiment provides a method for preparing a low-temperature solid-phase sintered self-synthesized MgAl2O4 ceramic, and its process is the same as that of Example 4, except that in this embodiment, in S5, the temperature is finally raised from 1000°C to 1500°C at 5°C / min and kept at this temperature for 3 hours, and then cooled to room temperature with the furnace to obtain a high thermal conductivity and high strength MgAl2O4 ceramic.

[0060] Example 8

[0061] The present embodiment provides a method for preparing a low-temperature solid-phase sintered self-synthesized MgAl2O4 ceramic, and its process is the same as that of Example 3, except that in this embodiment, in S5, the temperature is finally raised from 1000°C to 1480°C at 5°C / min and kept for 3 hours, and then cooled to room temperature with the furnace to obtain a high thermal conductivity and high strength MgAl2O4 ceramic.

[0062] Example 9

[0063] The present embodiment provides a method for preparing a low-temperature solid-phase sintered self-synthesized MgAl2O4 ceramic, and its process is the same as that of Example 3, except that in this embodiment, in S5, the temperature is finally raised from 1000°C to 1530°C at 5°C / min and kept for 3 hours, and then cooled to room temperature with the furnace to obtain a high thermal conductivity and high strength MgAl2O4 ceramic.

[0064] Comparative Example 1

[0065] This embodiment provides a method for preparing low-temperature solid-phase sintering self-synthesized MgAl2O4 ceramics, the steps comprising:

[0066] S1. Using anhydrous ethanol as dispersant and Al2O3 balls as grinding media, mix Al2O3 and MgO powders in a mass ratio of 71.8:28.2 and put them into a corundum ball mill at a speed of 280r / min for 6h to fully mix the raw materials.

[0067] S2. Pour the ball-milled mixture into an evaporating dish, and place the evaporating dish in a constant temperature oven for drying. The oven temperature is set at 50°C. After it is completely dried, take out the raw material, gently scrape it into the sieve with a medicine spoon, and continue to grind until the raw material completely passes through the 80-mesh sieve to form a mixed powder.

[0068] S3. Mechanically mix the mixed powder with the alkaline solution, then age it, add the organic monomers acrylic acid (AA), N,N-dimethylacrylamide (DMAA), crosslinker N,N-methyleneacrylamide (MBAM), dispersant PEG400, PEG1000, and ammonium polyacrylate (NH4PAA) into water for full dissolution and mixing, so that the powder forms a gel liquid, and add initiators potassium persulfate and sodium persulfate, and catalyst tetramethylethylenediamine into the gel liquid. Finally, inject and solidify it into a sheet to obtain a green body with high strength and a bending strength of 20-40MPa.

[0069] S4. Dehydrate the green body at 50-100℃ to slowly remove the water in the green body. Then, heat the green body from 100℃ to 1000℃ at 5℃ / min, and keep the temperature at 400℃ and 800℃ for 2h respectively to ensure complete degreasing.

[0070] S5. Finally, the temperature was raised from 1000°C to 1550°C at a rate of 5°C / min and kept at that temperature for 3 hours, and then cooled to room temperature in the furnace to obtain MgAl2O4 ceramics.

[0071] The MgO ceramic materials prepared in Examples 1 to 7 and Comparative Examples 1 and 2 were tested for performance, and the test results are shown in Table 1 below:

[0072] Table 1

[0073]

[0074]

[0075] It can be seen from Table 1 that as the amount of TiO2 added increases, its density, thermal conductivity and flexural strength show an upward trend, and a better density and flexural strength are obtained at a content of 3%. Figure 1 It can be seen that with the addition of TiO2, the diffraction peak height of MgAl2O4 gradually increases, which can be inferred that more and more MgAl2O4 phase is synthesized by the reaction. Figure 2It can be seen that at 1550℃, the density of the sample gradually increases, and the intergranular gap gradually decreases, but the grain size of the 4% content is not much different from that of the 3% content. When the optimal TiO2 addition amount of the present invention is 3%, the sintering at 1480℃, 1500℃, 1530℃ and 1550℃ is respectively: Figure 3 It can be seen that, for the sample with 3% content, as the temperature increases, the liquid phase generated by the reaction gradually increases, the grain gap gradually becomes smaller, and the density of the sample becomes better and better.

[0076] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing low-temperature solid-phase sintering self-synthesized MgAl2O4 ceramics, characterized in that: The preparation steps include: S1. The aluminum oxide, magnesium oxide and titanium dioxide powders are mixed uniformly in a mass ratio to obtain a mixed powder; S2. The mixed powder is mixed with an alkaline solution, aged, and then an organic matter is added to form a gel-like liquid and cross-linked to form a body; S3. The green body is dehydrated at 50 to 100 ° C, and then heated to 1000 ° C for degreasing; S4. The degreased green body is heated to 1480-1550° C. for sintering, and the MgAl 2 O 4 ceramic material is obtained after cooling.

2. The method for preparing low temperature solid phase sintering self-synthesized MgAl2O4 ceramics according to claim 1, characterized in that: The mass ratio of aluminum oxide to magnesium oxide is 70-75:25-30.

3. The method for preparing low temperature solid phase sintering self-synthesized MgAl2O4 ceramics according to claim 1, characterized in that: The addition amount of the titanium dioxide is 1-4% of the total mass of the aluminum oxide and the magnesium oxide.

4. The method for preparing low temperature solid phase sintering self-synthesized MgAl2O4 ceramics according to claim 1, characterized in that: The mixed powder is pre-treated by ball milling.

5. The method for preparing low temperature solid phase sintering self-synthesized MgAl2O4 ceramics according to claim 1, characterized in that: The mass ratio of the mixed powder to the organic matter is 2 to 4:

1.

6. The method for preparing low temperature solid phase sintering self-synthesized MgAl2O4 ceramics according to claim 1, characterized in that: The organic matter includes monomers, cross-linking agents, initiators and catalysts.

7. The method for preparing low temperature solid phase sintering self-synthesized MgAl2O4 ceramics according to claim 7, characterized in that: The monomer is one or more of acrylic acid, dimethyl acrylamide, dimethylamino methacrylate, methacrylate, and hydroxyethyl acrylate; the crosslinking agent is one or more of N,N-methylene acrylamide and isocyanate; the initiator includes one or more of persulfates, tert-butyl hydroperoxide, sodium pyrosulfite, and sucrose; the catalyst is one or more of tetramethylethylenediamine, Lewis acid, and polyacrylamide.

8. The method for preparing low temperature solid phase sintering self-synthesized MgAl2O4 ceramics according to claim 1, characterized in that: The heating degreasing temperature rise stage includes: heating from 100°C to 200-400°C, keeping the temperature for 2-3 hours, then heating to 420-800°C, keeping the temperature for 2-3 hours, and finally heating to 1000°C and keeping the temperature for 1-2 hours to complete the degreasing.

9. The method for preparing low temperature solid phase sintering self-synthesized MgAl2O4 ceramics according to claim 1, characterized in that: The heating rate of the degreasing process is 3-6°C / min.

10. The method for preparing low temperature solid phase sintering self-synthesized MgAl2O4 ceramics according to claim 1, characterized in that: The heating rate of the sintering is 3-6°C / min, and the heat preservation time of the sintering is 2-3h.

Citation Information

Patent Citations

  • Magnesia-alumina spinel material prepared by waste activated alumina and preparation method thereof

    CN101580383A

  • Preparation method of fine-grain broadband magnesium aluminate spinel transparent ceramic

    CN106747399A

  • Preparation method of Si3N4 heat-conducting ceramic material

    CN113831140A

  • Corundum-magnesium aluminate spinel multiphase heat storage ceramic and preparation method thereof

    CN117105639A

  • Spinel forming refractory compositions, their method of production and use thereof

    US20160122249A1