Zero-dimensional hybrid lead-free metal halide materials, their preparation methods and applications
By doping Sb3+ in [Im-BDMPA]InCl6·H2O, an efficient [Im-BDMPA]In0.78Sb0.22Cl6·H2O material was prepared, which solved the problem of photoluminescence and radioluminescence of existing zero-dimensional hybrid halide materials. Solving the problem of insufficient performance, it achieves efficient photoluminescence and X-ray scintillation performance and is suitable for a variety of optoelectronic applications.
Patent Information
- Application Number
- CN202310228072.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-10
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-03-10
AI Technical Summary
Existing zero-dimensional hybrid halide materials have shortcomings in photoluminescence and radioluminescence properties, especially low light quantum yield, which makes them unable to serve as efficient X-ray detection materials.
Using [Im-BDMPA]InCl6·H2O and Sb-doped [Im-BDMPA]In0.78Sb0.22Cl6·H2O materials, they are prepared by wet chemical or mechanical grinding solid-state reaction methods, combined with the doping of Sb3+, to achieve efficient light Luminescent and radioluminescent properties.
Achieved high optical quantum yield close to 100%, broadband yellow light emission with large Stokes shift, significantly improved X-ray scintillation performance and sensitivity and selectivity of fluorescent probes, suitable for white light-emitting diodes, X-ray scintillation and fluorescence sensor field.
Smart Images

Figure CN116554037B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of luminescent materials, and in particular to a zero-dimensional hybrid lead-free metal halide material and a preparation method and application thereof. Background Art
[0002] In the past few decades, CsPbX3 (X=Cl, Br or I) halide perovskite nanocrystals (PNCs) have replaced traditional crystalline materials and become a new generation of optoelectronic functional materials due to their many excellent optical and electronic properties such as wide band gap, high absorption coefficient, low defect density, and long carrier diffusion length. In particular, PNCs have excellent luminescence properties such as tunable emission wavelength covering the entire visible spectrum, narrow half-peak width, and high quantum yield. And because of their high quantum efficiency and wide color gamut display range, three-dimensional PNCs have been explored and become down-conversion phosphors to prepare advanced optical devices such as solid-state light-emitting diodes and backlit liquid crystal displays. Since 2018, 3D PNCs have been identified as new scintillating materials due to their strong X-ray absorption and conversion capabilities, and have been further studied in X-ray detection and imaging applications. In addition, the diverse crystal structure and dynamic ionic properties also give 3D PNCs reversible photoluminescence conversion capabilities, allowing them to be used as fluorescent sensors in response to external stimuli. Therefore, 3D PNCs have broad application prospects in advanced optical fields such as light-emitting diodes, photovoltaic cells, photodetectors, lasers, scintillators and fluorescent probes. However, despite the excellent optoelectronic properties of 3D PNCs, their emission spectrum instability and lead ion toxicity still seriously restrict their application in industrial production. Therefore, in-depth research and exploration of new environmentally friendly perovskite derivatives are of great significance.
[0003] Recently, zero-dimensional organic-inorganic hybrid metal halide perovskites have attracted great attention due to their excellent optoelectronic properties and outstanding stability, and have become one of the candidate materials that can replace three-dimensional PNCs. In fact, multifunctional organic species and a large amount of non-toxic metal ions (Cu + , Mn 2+ 、Zn 2+ 、In 3+ , Sb 3+etc.) endow hybrid metal halides with diversified structures and excellent luminescence properties. In particular, the strong quantum confinement and highly localized electrons within the lattice can often lead to a substantial increase in the binding energy of excitons, thus giving them a high quantum yield. Importantly, the soft lattice in zero-dimensional metal halides easily vibrates strongly with light-induced excitons, thereby forming a strong electron-phonon coupling effect, which further produces broadband spectral emission with a large Stokes shift. Therefore, these zero-dimensional hybrid metal halides can be used as down-conversion phosphors to manufacture white light-emitting diodes. More importantly, zero-dimensional hybrid metal halides have been further explored and become X-ray scintillating materials due to their high quantum yields and large Stokes shifts. For example, based on Mn 2+ and Cu + Zero-dimensional metal halides show extraordinary scintillation properties, with light yields exceeding 80,000 photons MeV -1 , which is much better than typical CsPbX3 PNCs (about 21,000 photons MeV -1 )、CsI:Tl(54,000 photons MeV -1 ) and Gd2O2S:Tb(60,000 photons MeV -1 ) and other commercial scintillators. In addition, the softer lattice also gives zero-dimensional metal halides more opportunities to accommodate or recognize small molecules with changes in luminescence properties, making them potential as highly selective and sensitive fluorescent probes. Therefore, zero-dimensional hybrid metal halides provide an excellent structural platform for achieving ideal luminescence properties and preparing a variety of advanced optoelectronic applications. There is no doubt that ultra-high quantum yield and large Stokes shift are crucial for zero-dimensional hybrid halides to be used as down-conversion phosphors or X-ray scintillators.
[0004] Among the many zero-dimensional hybrid metal halides, indium-based halides have [InX4] - 、[InX5] 2- and [InX6] 3- It has been considered as one of the most promising luminescent materials due to its diverse coordination structures, non-toxicity, and high oxidation resistance. 2+ Almost fixed green or red emission of base halides, Sb 3+ Yellow to orange emission from halides and Zn 2+Compared with the blue emission of halides, zero-dimensional indium-based halides have multiple advantages such as adjustable emission wavelength covering the entire visible spectrum and large Stokes shift. They have been proven to be able to be used as fluorescent probes to make reversible luminescence switching in response to external chemical stimuli such as water and methanol. Unfortunately, so far, no zero-dimensional hybrid indium halide can serve as an X-ray detection material due to its low light quantum yield. These shortcomings have inspired people to design and synthesize new zero-dimensional indium halides through crystal engineering at the molecular level to achieve efficient photoluminescence and radiative luminescence efficiency. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a zero-dimensional hybrid lead-free metal halide material and a preparation method and application thereof. The prepared zero-dimensional hybrid lead-free metal halide material has excellent photoluminescence, radioluminescence and detection performances.
[0006] The technical solution of the present invention is:
[0007] In a first aspect, the present invention provides a zero-dimensional hybrid lead-free metal halide material, wherein the molecular formula of the zero-dimensional hybrid lead-free metal halide material is [Im-BDMPA]InCl6·H2O, wherein Im-BDMPA is 3,3′-iminobis(N,N-dimethylpropylamine), the crystal system space group is P212121, and the unit cell parameter is α=β=γ=90°, Z=4, the unit cell volume is
[0008] Preferably, the zero-dimensional hybrid lead-free metal halide material is doped with antimony element, and the molecular formula of the obtained material is [Im-BDMPA]In 0.78 Sb 0.22 Cl6·H2O.
[0009] In a second aspect, the present invention provides a method for preparing the above-mentioned zero-dimensional hybrid lead-free metal halide material, comprising adding InCl3·4H2O and 3,3′-imidobis(N,N-dimethylpropylamine) to a mixed solution of hydrochloric acid, isobutanol and acetonitrile, heating and stirring to dissolve; transferring and sealing the solution in a reactor, heating at 80-105°C for at least 5 days, and then cooling to room temperature to obtain crystals; washing the crystals with methanol, and filtering to obtain the zero-dimensional hybrid lead-free metal halide material.
[0010] Preferably, the molar ratio of InCl3·4H2O to 3,3′-iminobis(N,N-dimethylpropylamine) is 1:(2-3).
[0011] Preferably, the volume ratio of hydrochloric acid, isobutanol and acetonitrile is 1:(1-2):(1-3).
[0012] Preferably, the solution is dissolved by heating at 40-50°C and stirring.
[0013] Preferably, SbCl3, InCl3·4H2O and 3,3′-imidobis(N,N-dimethylpropylamine) are added together into a mixed solution of hydrochloric acid, isobutyl alcohol and acetonitrile, and a zero-dimensional hybrid lead-free metal halide material doped with antimony element is obtained under the same reaction conditions.
[0014] Preferably, the molar ratio of SbCl3 to InCl3·4H2O and 3,3′-iminobis(N,N-dimethylpropylamine) is (1-1.5):1:(2-3).
[0015] In a third aspect, the present invention further provides an application of the above zero-dimensional hybrid lead-free metal halide material, wherein the zero-dimensional hybrid lead-free metal halide material is applied to the fields of white light emitting diodes, X-ray scintillation and fluorescence sensors.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] 1. This invention focuses on the field of solid-state white light emitting diodes and X-ray scintillators, aiming to explore zero-dimensional hybrid indium halide materials with high-efficiency luminescence and multifunctional optoelectronic applications. This invention uses a simple wet chemical or mechanical grinding solid phase reaction method based on discrete [InCl6] 3- A new zero-dimensional hybrid indium halide [Im-BDMPA]InCl6·H2O was prepared by octahedron; in addition, the present invention also uses a reasonable Sb 3+ Doping, [Im-BDMPA]In 0.78 Sb 0.22 Cl6·H2O has a quantum yield close to 100% in all states in single crystals, nanoparticles, and flexible films, and exhibits efficient broadband yellow light emission with a Stokes shift of 1.28 eV. 3+ [Im-BDMPA]In 0.78 Sb 0.22 Cl6·H2O shows extraordinary X-ray scintillation performance with a light yield of up to 55320 photons MeV -1 , which is the first indium halide-based X-ray scintillator. At the same time, this zero-dimensional hybrid indium halide also represents the first perovskite material as a unique fluorescent probe with ultra-high sensitivity, selectivity and repeatability. In general, the zero-dimensional halides prepared by this invention show a variety of optoelectronic applications in white light emitting diodes, X-ray scintillators and fluorescent sensors. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1Schematic diagram of the crystal structure of the compound obtained in Example 1 of the present invention, wherein Figure a is a schematic diagram of the assembly of Compound 1; Figure b is a schematic diagram of the zero-dimensional structure of Compound 1; Figure c is an X-ray diffraction diagram of the compounds obtained in Examples 1 and 2;
[0019] Figure 2 The scanning electron microscope photo a, energy scattering spectrum b and element spectrum c of the compound crystal prepared in Example 1 of the present invention;
[0020] Figure 3 The scanning electron microscope photo (Figure a), energy scattering spectrum (Figure b), and elemental spectrum (Figure c) of the compound crystal prepared in Example 2 of the present invention;
[0021] Figure 4 This is a scanning electron microscope photograph of the compound nanoparticles prepared in Example 3 of the present invention;
[0022] Figure 5 The X-ray diffraction pattern of the crystal prepared in Example 2 of the present invention (Figure a), the X-ray diffraction pattern of the suspension prepared in Example 2 (Figure b) and the X-ray diffraction pattern of the film prepared in Example 2 (Figure c);
[0023] Figure 6 Specific luminescence characterization diagrams of the crystal prepared in Example 1 of the present invention, wherein Figure (a) is the CIE coordinates corresponding to the crystal; Figure (b) is the excitation and emission spectra of the crystal; Figure (c) is the luminescence lifetime of the crystal at 80K and 300K; Figure (d) is the emission spectrum of the crystal under different excitation powers; Figure (e) is the power-dependent emission spectrum of the crystal;
[0024] Figure 7 The excitation lifetime of the crystal prepared in Example 1 of the present invention at 450nm;
[0025] Figure 8 The photoluminescence spectra of the products prepared in Examples 2-4 of the present invention are shown in Figure a, wherein Figure a is the photoluminescence spectrum corresponding to the crystal prepared in Example 2; Figure b is the photoluminescence spectrum corresponding to the suspension prepared in Example 3; and Figure c is the photoluminescence spectrum corresponding to the film prepared in Example 4;
[0026] Fig. 9 The photoluminescence quantum yields of the crystals prepared in Examples 1-2 of the present invention, wherein Figure a is the photoluminescence quantum yield of the crystals prepared in Example 1; Figure b is the photoluminescence quantum yield of the crystals prepared in Example 2;
[0027] Fig.10 The luminescence lifetime of the crystal prepared in Example 1 of the present invention;
[0028] Fig.11The three-dimensional fluorescence spectra of the crystals prepared in Examples 1-2 of the present invention, and the corresponding emission and excitation spectra under different excitations and different emissions, wherein Figure a is the three-dimensional fluorescence spectrum of the crystal of Example 1; Figure b is the excitation spectrum under different emission wavelengths corresponding to the crystal of Example 1; Figure c is the emission spectrum under different excitations corresponding to the crystal of Example 1; Figure e is the three-dimensional fluorescence spectrum of the crystal of Example 2; Figure f is the excitation spectrum under different emission wavelengths corresponding to the crystal of Example 2; Figure g is the emission spectrum under different excitations corresponding to the crystal of Example 2;
[0029] Fig.12 The crystal powder emission spectra of the crystals prepared in Examples 1-2 of the present invention, wherein Figure a is the crystal powder emission spectrum of the crystals prepared in Example 1; Figure b is the crystal powder emission spectrum of the crystals prepared in Example 2;
[0030] Fig.13 The luminescence characterization diagram of the crystal prepared in Example 2 of the present invention, wherein Figure a is the emission spectrum of the crystal depending on the excitation power; Figure b is the emission spectrum of the crystal under different excitation powers;
[0031] Fig.14 The orbital density diagram of the crystal prepared in Example 2 of the present invention is obtained by theoretical calculation, wherein Figure a is the orbital energy level diagram of the crystal; Figure b is the orbital density diagram of the crystal;
[0032] Fig.15 The thermogravimetric analysis spectra of the crystals prepared in Examples 1-2 of the present invention, wherein Figure a is the thermogravimetric analysis spectra of the crystals prepared in Example 1; Figure b is the thermogravimetric analysis spectra of the crystals prepared in Example 2;
[0033] Fig.16 This is a thermal stability test of the crystal prepared in Example 2 of the present invention, wherein Figure a is a comparison diagram of the powder diffraction patterns of the crystal after heating; Figure b is a comparison curve diagram of the emission intensity of the crystal at different temperatures;
[0034] Fig.17 This is a test of the stability of the crystal prepared in Example 2 of the present invention in a humid environment, wherein Figure a is a powder X-ray diffraction diagram of the crystal after being placed in a humid environment for one month; Figure b is a comparison curve diagram of the emission spectrum of the crystal after being placed in a humid environment for one month;
[0035] Fig.18 The photoluminescence spectrum of the crystal prepared in Example 2 of the present invention after being mixed with phosphors of different mass ratios under 365nm excitation, wherein the mass ratio of the crystal to the phosphor is 1:1, 1:1.13, 1:1.14, 1:1.16, 1:1.18, 1:1.2, 1:1.22, 1:1.23;
[0036] Fig.19CIE coordinates of the crystals prepared in Example 2 of the present invention mixed with phosphor powders in different proportions, wherein the weight ratios of the crystals to the phosphor powders are 1:1, 1:1.13, 1:1.14, 1:1.16, 1:1.18, 1:1.2, 1:1.22, and 1:1.23, respectively;
[0037] Fig. 20 The electroluminescence spectrum of the white light LED made from the crystal prepared in Example 2 of the present invention (Figure a) and the CIE coordinates of the white light LED (Figure b);
[0038] Fig.21 The electroluminescence spectra of the crystal prepared in Example 2 of the present invention at different driving currents;
[0039] Fig. 22 The electroluminescent emission spectrum of the white light LED made of the crystal prepared in Example 2 of the present invention that changes with time (Figure a) and the curve of the change of luminous efficiency with time (Figure b);
[0040] Fig.23 The radioluminescence spectra of the crystals prepared in Examples 1-2 of the present invention and commercial Ce:LuAG under X-rays;
[0041] Fig.24 The relevant tests of the X-ray scintillation performance of the crystal prepared in Example 2 of the present invention, wherein Figure a is a comparison curve of the absorption coefficient of the crystal and the standard sample Ce:LuAG; Figure b is the mechanism of X-ray excitation; Figure c is the radioluminescence spectrum of the crystal under different radiation doses; Figure d is the relationship between the radiation dose rate and the radioluminescence intensity of the crystal; Figure e is the stability of the crystal under continuous X-rays;
[0042] Fig.25 The screen of the crystal prepared in Example 2 of the present invention is used for X-ray imaging under 50 kV X-ray irradiation, wherein Figures ae are X-ray imaging photos of the sample, and the samples in Figures ae are respectively a lamp tube, a ballpoint pen, a chip, a power plug and a scale plate; Figure f is the spatial resolution of the crystal; Figure g is a comparison of the spatial resolution of the crystal and the commercial sample; Figure h is the afterglow curve of the crystal after the X-ray is turned off;
[0043] Fig.26The application of the film prepared in Example 4 of the present invention in the field of fluorescent probes, wherein Figure a is the emission spectrum of the film in different solvents; Figure b is a comparison diagram of the emission intensity of the film in different solvents; Figure c is a comparison diagram of the emission intensity of the film under bromoform cycle; Figure d is a bar graph comparing the emission intensity of the film in a mixed solvent and bromoform solvent, wherein I to VIII correspond to chloroacetic acid, dichloroacetic acid, chloroform, dichloromethane, dibromochloromethane, dichloromethane, chloroform, a mixed solvent of dibromochloromethane and bromoform in a volume ratio of 1:1; Figure e is a graph showing the emission intensity of the film when exposed to a low concentration of bromoform (concentration of 10 -1 -10 -8 mol / L) solution; Figure f is the PL emission spectrum of the solution containing 2×10 -7 -9×10 -7 PL emission spectra of the films after being immersed in carbon tetrachloride solutions with different concentrations of bromoform (mol / L), where the inset in the upper right corner of Figure f is the linear fit between the emission intensity and the bromoform concentration;
[0044] Fig. 27 PL emission spectra of the thin film prepared in Example 4 of the present invention after being immersed in various organic solvents;
[0045] Fig.28 X-ray powder diffraction patterns of the thin film prepared in Example 4 of the present invention after being immersed in various organic solvents;
[0046] Fig.29 The powder diffraction pattern (Figure a) and emission spectrum (Figure b) of the film prepared in Example 4 of the present invention after being immersed in carbon tetrachloride and bromoform solution;
[0047] Fig.30 The XPS spectra of the film prepared in Example 4 of the present invention before and after being immersed in tribromoform (TBM), wherein Figure a is the XPS total spectrum of the film; Figure b is the XPS spectrum of Cl in the film; Figure c is the XPS spectrum of Sb in the film; and Figure d is the XPS spectrum of In in the film;
[0048] Fig.31 The photoluminescence spectra of the film prepared in Example 4 of the present invention in various organic solvents with volume concentrations of 0% and 1%, wherein the organic solvents corresponding to Figures ag are chloroform, dichloromethane, dibromochloromethane, dichloromethane, chloroform, dibromochloromethane and carbon tetrachloride, respectively.
[0049] Fig.32 The figure is the powder X-ray diffraction pattern of the compound prepared in Comparative Example 1 of the present invention.
[0050] Fig.33 The excitation spectrum and emission spectrum of the compound prepared in Comparative Example 1 of the present invention at 300K.
[0051] Fig.34 It is the quantum yield of the compound prepared in Comparative Example 1 of the present invention at 300K.
[0052] Fig.35 The figure is the powder X-ray diffraction pattern of the compound prepared in Comparative Example 2 of the present invention.
[0053] Fig.36 The excitation spectrum and emission spectrum of the compound prepared in Comparative Example 2 of the present invention at 300K.
[0054] Fig.37 It is the quantum yield of the compound prepared in Comparative Example 2 of the present invention at 300K. DETAILED DESCRIPTION
[0055] In order to enable persons skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention.
[0056] 1. Materials used in the following examples
[0057] The raw materials used in the embodiments are all provided by Aladdin Reagent Company: indium chloride tetrahydrate (purity 99.9%), antimony trichloride (purity 99.9%), 3,3′-iminobis(N,N-dimethylpropylamine) (i.e., Im-BDMPA) (purity 99%), ethanol, isobutanol, hydrochloric acid, acetone, acetonitrile, epoxy resin ab glue and crosslinking agent Sylgard 184 elastomer, polytetrafluoroethylene mold; the reaction container is a 25 mL glass bottle that can withstand temperatures below 120°C.
[0058] 2. Instruments and testing methods
[0059] The electric heating blast drying oven was provided by Shanghai Yiheng Scientific Instrument Co., Ltd., model DHG-9240(A).
[0060] The crystal structure was determined by single crystal X-ray diffractometer (SMART APEXII, Bruker, Germany).
[0061] The powder diffraction was measured by X-ray powder diffractometer (Bruker D8 ADVANCE), and the UV-visible absorption spectrum was measured by UV-visible spectrophotometer (PE Lambda 900).
[0062] PL spectroscopy was performed on an Edinburgh FLS980 fluorescence spectrometer.
[0063] The photoluminescence quantum yield was achieved by adding an integrating sphere to the FLS980 fluorescence spectrometer.
[0064] The thermal stability test was performed by thermogravimetric analysis (TGA) on a Mettler TGA / SDTA 851 thermal analyzer in the temperature range of 30-800°C under the constant protection of N2 atmosphere flow.
[0065] Elemental analysis was performed on a scanning electron microscope (SEM, Zeiss Merlin Compact); X-ray photoelectron spectroscopy (XPS) spectroscopy was performed at Escalab XI + Instrument tested; SEM and DEX images were taken on a Hitachi SU-8010 field emission scanning electron microscope.
[0066] Inductively coupled plasma optical emission spectrometry (ICP-OES) measurements were performed on an Agilent 5110.
[0067] The contents of elements (C, N, H) were determined by elemental analysis (EA) on an Elemantar.
[0068] Example 1 Synthesis of [Im-BDMPA] InCl6·H2O
[0069] 1) Add InCl3·4H2O (1 mmol, 0.2932 g) and Im-BDMPA (1 mmol, 0.1873 g) to a mixed solution of 1 mL hydrochloric acid, 3 mL isobutyl alcohol and 2 mL acetonitrile, continue heating to 45°C and stirring to dissolve;
[0070] 2) transferring and sealing the solution into a 25 mL glass reactor, heating at a constant temperature of 80° C. for 5 days, and cooling to room temperature at a cooling rate of 5° C. / min to obtain crystals;
[0071] 3) Wash the crystals three times with methanol, collect the colorless plate-like crystals by filtration, and seal them for storage.
[0072] The molecular formula of the colorless plate-like crystals obtained is [Im-BDMPA]InCl6·H2O, the crystal system space group is P212121, and the unit cell parameters are α=β=γ=90°, Z=4, the unit cell volume is
[0073] The present invention prepares [Im-BDMPA]InCl6·H2O bulk single crystals by a typical low-temperature solvothermal method. According to single crystal X-ray diffraction, the [Im-BDMPA]InCl6·H2O crystal structure crystallizes in the orthorhombic space group P212121 and is composed of discrete [InCl6] 3- Octahedral and bulk [Im-BDMPA] 3+All the trivalent indium ions are surrounded by six chloride ions to form [InCl6] 3- octahedral, and the distance between the In-Cl bonds is within the normal range (such as Figure 1 a). All adjacent [InCl6] 3- The octahedrons are all long chains of [Im-BDMPA] 3+ The cations are separated and form a zero-dimensional halide structure at the molecular level (e.g. Figure 1 The matching degree between the experimental and simulated powder X-ray diffraction peaks demonstrates the purity and high crystallinity of the [Im-BDMPA]InCl6·H2O sample (as shown in Figure 2a). Figure 1 c). In addition, the present invention examines the distribution of chemical components by energy dispersive X-ray spectroscopy and elemental mapping (such as Figure 2 b-2c).
[0074] The photoluminescence spectrum of [Im-BDMPA]InCl6·H2O bulk single crystal shows a maximum peak around 564nm, a large Stokes shift of 294nm, and a wide Gaussian-shaped broadband yellow emission with a half-peak width of 138nm (e.g. Figure 6 b); the corresponding CIE coordinates are (0.39, 0.48) and are located in the yellow light area (such as Figure 6 Based on the biexponential function fitting, the time-resolved luminescence decay curve gives the average lifetime of 6.35μs (300K) and 12.78μs (80K) of the [Im-BDMPA]InCl6·H2O crystal prepared in Example 1 (as shown in Fig. Figure 6 c). In order to confirm its photoluminescence properties, the linear dependence between the crystal emission intensity and the excitation power obtained in Example 1 further excludes the existence of permanent crystal defects (such as Figure 6 de).
[0075] Example 2 [Im-BDMPA] In 0.78 Sb 0.22 Synthesis of Cl6·H2O
[0076] The preparation process is the same as that of Example 1, except that SbCl3 (1.5 mmol, 0.3453 g) is added to the mixed solution together with InCl3·4H2O (1 mmol) and Im-BDMPA (2 mmol). Finally, Sb-doped [Im-BDMPA]In 0.78 Sb 0.22 Cl6·H2O colorless crystals, yield 82%.
[0077] Sb 3+ Doped [Im-BDMPA]In0.78 Sb 0.22 The Cl6·H2O single crystal phase is obtained by adding the required amount of SbCl3 during the synthesis of the original single indium phase. The highly matched powder X-ray diffraction pattern shows that it has the same crystal structure as the single indium phase (such as Figure 1 c). At the same time, energy dispersive X-ray spectroscopy and elemental mapping further confirmed the chemical composition of the Sb-doped phase (e.g. Figure 3 ac), and the optimal doping concentration of Sb element was determined to be 22% by inductively coupled plasma optical emission spectroscopy (as shown in Table 1).
[0078] Table 1
[0079]
[0080] like Figure 6 a and Figure 8 As shown in a, the [Im-BDMPA]InCl6·H2O bulk single crystal prepared in Example 1 and the [Im-BDMPA]In doped with Sb element prepared in Example 2 0.78 Sb 0.22 Cl6·H2O bulk single crystals all show the same bright yellow light emission under ultraviolet light. Figure 6-8 The results show that [Im-BDMPA]InCl6·H2O and doped phase [Im-BDMPA]In 0.78 Sb 0.22 The photoluminescence properties of Cl6·H2O are basically the same in terms of emission position, luminescent color and powder diffraction pattern. Therefore, it is judged that the doped phase only improves its performance and does not change its internal structure. Therefore, the doped phase with better luminescence performance is used as an example for discussion below.
[0081] Example 3 [Im-BDMPA] In 0.78 Sb 0.22 Synthesis of Cl6·H2O Nanoparticles
[0082] 1) [Im-BDMPA]In prepared in Example 2 0.78 Sb 0.22 Cl6·H2O crystals were ground with an agate mortar and pestle for 5 h to obtain powder;
[0083] 2) dispersing the obtained powder in an ethanol solvent to obtain a suspension; placing the suspension in a microwave digestion furnace and heating it at a power of 500 W at room temperature (25° C.) for 20 h; and then obtaining nanoparticles by centrifugal separation;
[0084] 3) The obtained microparticles were washed with ethanol and dried in a vacuum dryer at 50°C for 30 h to obtain [Im-BDMPA]In0.78 Sb 0.22 Cl6·H2O nanoparticles.
[0085] High-quality [Im-BDMPA]In was synthesized by microwave irradiation-assisted mechanical exfoliation. 0.78 Sb 0.22 The Cl6-H2O nanoparticles are finally sized to be less than 5 μm and have a nearly cubic shape (e.g. Figure 4 The theoretical simulation and experimental diffraction peaks in the powder X-ray diffraction pattern are basically consistent, indicating that the crystallinity of the nanoparticles is very high (as shown in Figure 5 In addition, the powder X-ray diffraction pattern confirmed that [Im-BDMPA]In 0.78 Sb 0.22 Cl6-H2O nanoparticles have 100% purity, and this special property provides a simpler preparation method for preparing various optoelectronic devices.
[0086] Example 4 [Im-BDMPA] In 0.78 Sb 0.22 Preparation of Cl6·H2O Flexible Film
[0087] 1) Dissolve 1 mL of silicone elastomer (epoxy resin ab glue) and 2 mL of crosslinker (Sylgard 184 elastomer, Dow Corning) in 10 mL of acetone and stir at room temperature for 8 h to obtain a well-dispersed mixed solution;
[0088] 2) [Im-BDMPA]In prepared in Example 3 0.78 Sb 0.22 Cl6·H2O nanoparticles were added to the mixture and stirred for 15 h. The mixture was then poured into a polytetrafluoroethylene mold and placed in a vacuum oven and dried overnight at 50 °C to evaporate the solvent to obtain [Im-BDMPA]In 0.78 Sb 0.22 Cl6·H2O flexible film.
[0089] The film obtained by spin coating the suspension and nanoparticles in Example 3 also emits bright yellow light under ultraviolet light. The prepared flexible halide / polymer composite film also shows yellow luminescence under ultraviolet light. The specific photoluminescence properties are characterized by absorption, steady-state and time-resolved spectra, such as Figure 8 As shown in a, [Im-BDMPA]In prepared in Example 2 0.78 Sb 0.22 Cl6·H2O exhibits a broad scattering absorption band in the range of about 250-400nm, originating from 5s 2 -Sb 3+ Ion 1S0→ 3 P n The peak at about 220nm belongs to the self-absorption between energy bands. The excitation spectrum and absorption band cover the corresponding entire ultraviolet range, which shows the coincidence of electronic transition. [Im-BDMPA]In 0.78 Sb 0.22 The photoluminescence spectra of Cl6·H2O single crystals, nanoparticles and thin films all show a maximum peak around 570 nm, a large Stokes shift of 291 nm and a wide Gaussian-shaped broadband yellow emission with a half-peak width of 135 nm (e.g. Figure 8 ac).
[0090] Compared with the low photon quantum yield (48.46%) of the undoped Sb [Im-BDMPA] InCl6·H2O prepared in Example 1, the Sb prepared in Example 2 3+ Doped [Im-BDMPA]In 0.78 Sb 0.22 Cl6·H2O, the photon yield increased to 95.79% (such as Fig. 9 As shown), this is one of the highest photon yields of 0D hybrid indium halide / antimony. Based on the biexponential function fitting, the time-resolved luminescence decay curve gives the average lifetime of 7.85μs (300K) and 15.48μs (80K) for the [Im-BDMPA]InCl6·H2O crystal prepared in Example 1 (as shown in Figure 2). Fig.10 In order to confirm its photoluminescent properties, the present invention records the excitation and emission spectra at different wavelengths in the entire UV-visible spectrum. The excitation and emission spectra with no change in spectral shape indicate that both the doped phase and the undoped phase have a unique radiation pathway from a single excited state, which can also be verified by a dominant emission center in the three-dimensional spectrum (such as Fig.11 The crystals obtained in Example 2 have similar emission spectra and intensities to the powdered crystals after grinding, which eliminates the possibility that the surface defects lead to the broad emission band (such as Fig.12 In addition, the linear dependence between the emission intensity and the excitation power further excludes the existence of permanent crystal defects (such as Fig.13 shown).
[0091] Density functional theory calculations further revealed that [Im-BDMPA]In 0.78 Sb 0.22 The detailed luminescence mechanism of Cl6-H2O. Fig.15 As shown, [Im-BDMPA]In 0.78 Sb 0.22Cl6-H2O shows a narrow band with a band gap of 2.82 eV, indicating that the carriers are highly localized and there is no electronic interaction between neighboring species. The electron density map shows that the highest occupied molecular orbital (HOMO) and the lowest unoccupied molecular orbital (LUMO) are located at [In / SbCl6] 3- On the octahedron (such as Fig.14 The total state density in the compound and the state density of each component (as shown in a) Fig.14 b) shows that the valence band maximum (VBM) is composed of Sb-5p / Cl-3s orbitals, while the conduction band minimum (CBM) is contributed by the In-5s / Cl-3s mixed states (as shown in Fig. Fig.14 b). Therefore, each [In / SbCl6] 3- The octahedrons act as individual luminescent centers by trapping excitons to form self-trapped excitons and promoting the emission of self-trapped excitons.
[0092] In addition to efficient broadband light emission, [Im-BDMPA]InCl6·H2O and doped phase [Im-BDMPA]In 0.78 Sb 0.22 Cl6·H2O has sufficient structural and optical stability. According to thermogravimetric analysis, [Im-BDMPA]InCl6·H2O and [Im-BDMPA]In 0.78 Sb 0.22 Cl6·H2O bulk crystals can be stable to about 280℃ (such as Fig.15 As shown in Fig.16 As shown in the figure, when continuously heated at different temperatures from 80°C to 280°C, the spectral shape remains unchanged, the intensity decreases slightly, and the number of powder X-ray diffraction peaks is consistent with the simulated peaks, indicating that it has sufficiently strong thermal stability. Fig.17 As shown in Figure 2, after long-term storage in humid air for one month, [Im-BDMPA]In 0.78 Sb 0.22 Cl6·H2O still maintains high crystallinity and almost the same emission intensity.
[0093] [Im-BDMPA]In 0.78 Sb 0.22 The high efficiency and stable broadband yellow emission (half-peak width = 135 nm) of Cl6·H2O makes it suitable as a down-conversion phosphor for the preparation of white light-emitting diodes. In order to verify the feasibility of this application, [Im-BDMPA]In 0.78 Sb 0.22 Cl6·H2O as yellow phosphor and commercial blue phosphor BaMgAl 10 O 17 :Eu 2+ Mix in different proportions. Fig.18 As shown in the figure, the mechanically mixed phosphors show white light emission under 365nm ultraviolet light and exhibit a broadband electroluminescence spectrum consisting of blue and yellow double emission peaks. In addition, by finely controlling the mixing ratio of the two phosphors, adjustable luminescence from cold white light to warm white light is obtained, and the corresponding color temperature can be adjusted between 9520K and 3320K (such as Fig.19 ). Subsequently, a white light emitting diode was made by applying the mixed phosphor on the UV chip. Driven by a current of 20 mA, the LED emitted bright white light with a color temperature of 4590 K and CIE chromaticity coordinates of (0.35, 0.33) (as shown in Fig. 20 Its color rendering index (CRI) is 95.4, which is much higher than that of YAG:Ce based LEDs on the market. 3+ In order to test the reabsorption effect between the two corresponding phosphors, the electroluminescence spectra were measured at different operating currents (such as Fig.21 As shown in Figure 2 ). As the current increases from 20mA to 120mA, the electroluminescent emission intensity of the dual emission peaks increases linearly with the increase of the driving current, and there is no energy transfer between the two phosphors. This remarkable feature shows the potential application in high-power white light-emitting diodes. Finally, in order to evaluate the working stability of the prepared light-emitting diode, the present invention monitors the electronic luminescence emission spectrum and working time under a driving current of 20mA, as shown in Figure 2 . Fig. 22 As shown, it can be clearly seen that the electroluminescence spectrum remains unchanged and the luminous efficacy has no obvious degradation within the working time of 100h, which indicates the good light stability of the light-emitting diode.
[0094] The high quantum yield, wide emission half-peak width and large Stokes shift prove that [Im-BDMPA]In 0.78 Sb 0.22 Cl6·H2O has the potential to be used as an X-ray scintillator. First, the photon cross section data of [Im-BDMPA]In 0.78 Sb 0.22 The X-ray absorption spectra of Cl6·H2O and commercial Ce:LuAG in a wide range of photon energies (e.g. Fig.23 [Im-BDMPA]In 0.78 Sb 0.22 The X-ray attenuation efficiency of Cl6·H2O is comparable to that of Ce:LuAG in the medical digital radiography region (18-30keV). Under 30keV X-ray irradiation, [Im-BDMPA]In 0.78 Sb 0.22The bulk crystals of Cl6·H2O show bright yellow light, and the scintillation properties are studied using it as an example. Both the original phase and the doped phase show a broad radiative luminescence emission band centered at 570 nm, indicating that the emission band under ultraviolet light excitation follows the same radiative recombination pathway (e.g. Fig.24 According to previous studies, the photoelectric effect mainly originates from the interaction between phonons and electrons in the inner shell of atoms under X-rays, which produces electrons and holes with higher energy (such as Fig.24 b). The hot carriers generated by this interaction enter the valence band and conduction band edges as secondary electrons and holes through thermal relaxation and further release energy. 66 The RL emission intensity of H2O is lower than that of Ce:LuAG, but it is 3+ The X-ray response was greatly enhanced, and its light output reached about 2.2 times that of Ce:LuAG (such as Fig.24 By integrating the peak area of the radioluminescence emission spectrum, [Im-BDMPA]InCl6·H2O and [Im-BDMPA]In 0.78 Sb 0.22 The light yield of Cl6·H2O is about 23047 photons / MeV and 55320 photons / MeV (such as Fig.24 Importantly, [Im-BDMPA]In 0.78 Sb 0.22 The light yield of Cl6·H2O exceeds that of most advanced commercial scintillators, including CsI:Tl (54,000 photons / MeV), CsI:Na (41,000 photons / MeV), CdWO4 (20,000 photons / MeV), LYSO (33,200 photons / MeV), etc. In addition, the scintillation light yield is also better than that of most halide scintillators, such as three-dimensional CsPbBr3 (about 21,000 photons / MeV), (PPN)2SbCl5 (49,000 photons / MeV), Cs3MnI5 (33,600 photons / MeV), (DIET)3Cu3Br3 (20,000 photons / MeV), etc. Such excellent scintillation performance is related to high X-ray attenuation efficiency, near-unity PLQY and large Stokes shift.
[0095] In order to study the detection sensitivity of this zero-dimensional indium halide to X-rays, the present invention collects radiation emission spectra at different X-ray dose rates. Fig.24 c, [Im-BDMPA]In 0.78 Sb 0.22Cl6·H2O shows the same radioluminescence emission spectrum curve as photoluminescence, and its emission intensity increases monotonically in the range of dose rates from 4,101.5 μGy / s to 43,577.8 μGy / s. When the signal-to-noise ratio (SNR) is 3, the best linear fit between the radioluminescence emission intensity and the dose rate gives an ultra-low detection limit of 0.0853 μGy / s (e.g. Fig.24 d). In addition, the radiation stability to X-ray irradiation is also an important indicator for evaluating the performance of X-ray scintillators. Under continuous X-ray irradiation at a fixed dose rate of 37mGy / s, within 30h, [Im-BDMPA]In 0.78 Sb 0.22 The radiation emission intensity of Cl6·H2O exhibits negligible fluctuation and decay, showing strong stability to X-rays (e.g. Fig.24 e).
[0096] The combined advantages of high light yield, ultra-low detection limit and sufficient X-ray durability are the main advantages of [Im-BDMPA]In 0.78 Sb 0.22 The application of Cl6·H2O in X-ray imaging provides feasibility. As a proof of concept, the present invention adopts X-ray imaging engineering and uses [Im-BDMPA]In on an X-ray imaging optical system. 0.78 Sb 0.22 Cl6·H2O thin film, and a series of small devices were selected as the target objects. Fig.25 As shown in a, the packaged fuse tube containing the wire is exposed to X-ray illumination. The different X-ray absorption capabilities of the wire and the glass tube lead to a bright spatial intensity contrast, which is converted into an optical image by the scintillation screen with the help of a digital camera. 0.78 Sb 0.22 The Cl6·H2O screen clearly shows the optical image inside the wire. Similarly, when a ballpoint pen containing a metal spring, a metal device, and an electronic chip are exposed to X-rays, all the metal parts can be clearly seen on the scintillating screen with sufficient contrast (such as Fig.25 b-25d). In order to obtain the spatial resolution of the scintillator screen, a standard X-ray resolution test pattern plate was used for X-ray imaging, and the observation limit was above 10lp / mm (as shown in Fig.25 e). The modulation transfer function (MTF) of the scintillator screen is further used on the oblique edge X-ray image to obtain a more precise spatial resolution (as shown in Fig.25f). When MTF is equal to 0.2, the spatial resolution of the screen is extracted as 28.72lp / mm, which is significantly better than commercial CsI(Tl) (10lp / mm), CsPbBr3:Lu (16.8lp / mm), CsPbBr3:Eu (15lp / mm), BA2PbBr4:10%Mn (10.7lp / mm), Rb2AgBr3 (10.2lp / mm), MAPbBr3 (9.8lp / mm), CsCu2I3 (7.5lp / mm), etc. (as shown in Figure 2). Fig.25 g). Finally, it is important to measure the radioluminescence afterglow to assess image contrast, given that a long radioluminescence lifetime can lead to strong image lag or ghosting after X-ray shut-off. Fig.25 As shown in h, the emission intensity of the radioluminescence afterglow signal drops rapidly to zero within 0.48 ms after the X-ray excitation is stopped, proving that the film prepared by this sample has high imaging contrast. In general, the high spatial resolution and negligible afterglow monomer indicate that the [Im-BDMPA]In 0.78 Sb 0.22 The Cl6·H2O scintillation screen has excellent X-ray imaging performance.
[0097] The soft and unique zero-dimensional crystal structure of the halide scaffold inspired the present invention to further study its luminescence switching phenomenon in response to external stimuli as a fluorescent probe for various small chemical molecules. 0.78 Sb 0.22 The Cl6·H2O thin film (Example 4) was used as a platform to study the luminescent switch performance. It showed the same luminescent performance as the bulk crystal, but was more feasible in sensing applications. 0.78 Sb 0.22 The sensing performance of Cl6·H2O was investigated by monitoring the photoluminescence emission spectra before and after exposing the films to various organic solvents for several hours. Here, a series of small halogenated hydrocarbon molecules or derivatives were selected as sensing targets, including chloroacetic acid (CAA), dichloroacetic acid (DCAA), chloropropiophenone (CPP), dibromomethane (DBM), bromodichloromethane (BDCM), dichloromethane (DCM), trichloromethane (TCM), dibromochloromethane (DBCM), and tribromoform (TBM). The photographs of the films under UV light irradiation showed that the fluorescence was rapidly quenched by tribromoform in less than a second, while the other films still showed the same bright yellow emission. The detailed emission spectra showed that the luminescence intensity of the films in the TBM solvent was almost completely quenched, while the luminescence intensity in other organic solvents showed almost no change (such as Fig.26a and 26b). In order to further examine the selectivity of the sensor, a large number of organic solvents containing different functional groups were selected as comparison targets, including alcohol, acetonitrile, acetone, tetrahydrofuran, acetylacetone, aromatic hydrocarbons (such as benzene, dimethylbenzene, chlorobenzene, nitrobenzene), etc. Figure 27-28 As shown, [Im-BDMPA]In 0.78 Sb 0.22 The Cl6·H2O film shows the same broad yellow emission band as the freshly prepared sample, and the emission intensity is almost the same. These comparative experiments show that [Im-BDMPA]In 0.78 Sb 0.22 The fluorescence of Cl6·H2O is only quenched by TBM, but not by other organic solvents. In addition, the fluorescence of the film quenched by TBM can be restored to its original yellow emission after being washed with carbon tetrachloride (CTC), and the photoluminescence emission intensity can reach nearly 100% of the original data (such as Fig.29 shown).
[0098] In order to more accurately confirm the repeatability of the reversible quenching-recovery process, the present invention monitored [Im-BDMPA]In 0.78 Sb 0.22 Different photoluminescence emission intensities of Cl6·H2O films during continuous immersion-washing cycles. The film shows reproducible luminescence quenching-recovery cycles, and the luminescence can be continuously restored to its original yellow color even after 20 consecutive cycles. At the same time, the decrease in emission intensity is negligible, which also indicates high reversibility and repeatability (e.g. Fig.26 c). After exposure to these organic solvents, the powder diffraction pattern shows strong diffraction peaks with high crystallinity, and the XPS spectrum is consistent with the synthetic data, indicating that the crystal structure lattice is stable (such as Fig.28 and Fig.30 Therefore, [Im-BDMPA]In 0.78 Sb 0.22 Cl6·H2O showed reversible TBM-responsive fluorescence on / off, which provided the feasibility of using it as a fluorescent probe to detect TBM.
[0099] The sharp contrast in the response to TBM and other organic solvents inspired the study of the selectivity of the present invention for sensing applications. The present invention conducted anti-interference experiments in a mixed solution of TBM and other halogenated hydrocarbon solvents to study the selectivity of detecting TBM. Fig.31 and 25 As shown in d, in the mixed solution containing a small amount of TBM (1% by volume), the PL emission intensity of the film is almost completely extinguished, but it fails in the solution without TBM, which indicates that [Im-BDMPA]In 0.78 Sb 0.22Cl6·H2O has excellent sensing selectivity for TBM. The sensitivity of the fluorescent probe is another key indicator for evaluating the sensing performance in practical applications. In order to explore the sensitivity of the fluorescent probe, a series of TBM / CTC solutions with very low concentrations were further mixed, ranging from 10 -1 -10 -8 mol / L is used as a representative target. Fig.26 As shown in e, the PL emission spectrum shows that when the TBM content is reduced to 10 -7 (0.1ppm), the film still showed quenching. -7 Up to 9×10 -7 mol / L, the detailed emission spectra of ultra-dilute TBM / CTC solutions showed that the fluorescence intensity of the film gradually decreased with the increase of TBM concentration, while the quenching effect (I0 / I -1 ) is linearly related to TBM concentration (R 2 =0.9998), indicating that the film has good detection operability (such as Fig.26 These results indicate that [Im-BDMPA]In 0.78 Sb 0.22 Cl6·H2O has high selectivity and sensitivity in detecting TBM and is an ideal fluorescent probe.
[0100] Comparative Example 1
[0101] The difference from Example 2 is that the molar ratio of SbCl3 to InCl3·4H2O and 3,3′-iminobis(N,N-dimethylpropylamine) is 2:1:2.
[0102] The compound prepared in Comparative Example 1 was determined to have a Sb doping concentration of 30% by inductively coupled plasma optical emission spectroscopy (as shown in Table 2). Therefore, the molecular formula of the prepared compound is [Im-BDMPA]In 0.70 Sb 0.30 Cl6·H2O.
[0103] Table 2
[0104]
[0105] like Fig.32 As shown, the powder diffraction pattern of the compound prepared in Comparative Example 1 is consistent with the data of the single crystal structure simulation, indicating that the purity of the compound prepared in Comparative Example 1 is close to the theoretical value (100%). Fig.33 As shown, the compound prepared in Comparative Example 1 has narrow excitation and emission spectra, with main peaks at 364 and 490 nm, respectively, a half-peak width of 78 nm and a Stokes shift of 126 nm. Fig.34As shown, the quantum yield of the compound prepared in Comparative Example 1 is 13.78%, which is much lower than that in Example 2. Therefore, it can be seen from Example 2 and Comparative Example 1 that different Sb doping concentrations and different molecular formulas of the prepared compounds will greatly affect the performance of the final prepared compound; when the Sb doping concentration is 22%, the prepared [Im-BDMPA]In 0.78 Sb 0.22 Cl6·H2O has the best performance.
[0106] Comparative Example 2
[0107] The difference from Example 2 is that in step 1), acetonitrile is used as the organic solvent.
[0108] The compound prepared in Comparative Example 2 has a doping concentration of Sb element of 40% as determined by inductively coupled plasma optical emission spectroscopy (as shown in Table 3), so the molecular formula of the prepared compound is [Im-BDMPA]In 0.6 Sb 0.4 Cl6·H2O.
[0109] Table 3
[0110]
[0111] like Fig.35 As shown, the powder diffraction pattern of the compound prepared in Comparative Example 2 is consistent with the data of the single crystal structure simulation, indicating that the purity of the compound prepared in Comparative Example 2 is close to the theoretical value (100%). Fig.36 As shown, the compound prepared in Comparative Example 2 has narrow excitation and emission spectra, with main peaks at 280 nm, 361 nm and 610 nm, respectively, and a half-peak width of 245 nm and a Stokes shift of 330 nm. Fig.37 As shown, the quantum yield of the compound prepared in Comparative Example 2 is 25.25%, which is much lower than that in Example 2. Therefore, it can be seen from Example 2 and Comparative Example 2 that the type of organic solvent will also affect the Sb-doped [Im-BDMPA]In 0.78 Sb 0.22 Preparation and properties of Cl6·H2O.
[0112] In summary, the present invention demonstrates a new zero-dimensional hybrid indium halide as an efficient broadband yellow light emitter with nearly uniform quantum yield and multifunctional optoelectronic applications. First, the broadband emission realizes high-performance white light emitting diodes with adjustable color temperature. Second, the halide is the first X-ray scintillating material among zero-dimensional hybrid indium halides, with outstanding light yield, extremely low detection limit, ultra-high spatial resolution and negligible afterglow time, and has good application prospects in X-ray imaging. Third, the reversible tribromoform-responsive luminescence switch makes it a perfect real-time fluorescent probe with ultra-high sensitivity, selectivity and repeatability. Therefore, the present invention simultaneously realizes high-performance multiple optoelectronic applications of white light emitting diodes, X-ray scintillating and fluorescent sensors on a zero-dimensional hybrid halide structure platform. These multiple applications benefit from intrinsic quantum confinement, strong electron-phonon coupling, sufficiently strong X-ray absorption coefficient and significant structural synergy in deformable lattices. This work not only deepens the basic understanding of the luminescence properties of zero-dimensional hybrid halides, but also realizes multiple optoelectronic applications. It is believed that this research will further guide people to rationally design new zero-dimensional hybrid metal halides as advanced luminescent materials in the cutting-edge optoelectronic field.
[0113] Although the present invention has been described in detail by referring to the accompanying drawings and in combination with the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person skilled in the art who is familiar with the present technical field can easily think of changes or substitutions within the technical scope disclosed by the present invention, and all of these shall be within the scope of protection of the present invention. Therefore, the scope of protection of the present invention shall be subject to the scope of protection of the claims.
Claims
1. A zero-dimensional hybrid lead-free metal halide material, characterized in that: The molecular formula of the zero-dimensional hybrid lead-free metal halide material is [Im-BDMPA]In 0.78 Sb 0.22 Cl6·H2O, which is obtained by doping antimony element in [Im-BDMPA]InCl6·H2O material, wherein Im-BDMPA is 3,3′-iminobis(N,N-dimethylpropylamine), and the crystal system space group is P2 1 2 1 2 1. Unit cell parameters a = 9.348(2) Å, b = 12.342(3) Å, c = 18.180(4) Å, α = β= γ = 90°, Z = 4, the unit cell volume is V = 2097.48 Å 3 .
2. The method for preparing the zero-dimensional hybrid lead-free metal halide material according to claim 1, characterized in that: SbCl3, InCl3·4H2O, and 3,3′-imidobis(N,N-dimethylpropylamine) are added together into a mixed solution of hydrochloric acid, isobutanol, and acetonitrile, and heated and stirred to dissolve; the solution is transferred and sealed in a reactor, heated at 80-105°C for at least 5 days, and then cooled to room temperature to obtain crystals; the crystals are washed with methanol, and filtered to obtain a zero-dimensional hybrid lead-free metal halide material; the volume ratio of hydrochloric acid, isobutanol, and acetonitrile is 1:(1-2):(1-3); the molar ratio of SbCl3, InCl3·4H2O, and 3,3′-imidobis(N,N-dimethylpropylamine) is (1-1.5):1:(2-3).
3. The use of the zero-dimensional hybrid lead-free metal halide material according to claim 1, characterized in that: The zero-dimensional hybrid lead-free metal halide material is applied in the fields of white light emitting diodes, X-ray scintillation and fluorescence sensors.