Method for synthesizing formamidine iodide using anion exchange resin as ion exchange medium
Through the anion exchange resin replacement reaction and NaI or KI as the iodine source, the safety hazards of hydriodic acid and the difficulty of separation of by-products are solved, and the industrial production of high-purity formamidine iodide is achieved.
Patent Information
- Application Number
- CN202310549991.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-05-16
AI Technical Summary
In the industrial production of perovskite photovoltaic materials, there are safety risks in using hydriodic acid to synthesize formamidine iodide, and when sodium iodide or potassium iodide is used directly, the by-product sodium acetate or potassium acetate and the product formamidine iodide are difficult to separate.
Anion exchange resin is used as the ion exchange medium, and the Cl-type anion exchange resin is replaced with I-type, and NaI or KI is used as the iodine source, combined with formamidine acetate for a displacement reaction, to achieve the synthesis and separation of formamidine iodide.
The safety hazard of using hydriodic acid is avoided, effective separation of formamidine iodide and by-products is achieved, and high-purity formamidine iodide is prepared, which is suitable for industrial large-scale production.
Smart Images

Figure CN116554058B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of synthesis of formamidine iodide, a precursor of a perovskite photovoltaic material, and specifically relates to a method for synthesizing formamidine iodide by using an anion exchange resin as an ion exchange medium and potassium iodide or sodium iodide as an iodine source. Background Art
[0002] Formamidine iodide is a precursor material for the perovskite light absorption layer, and its synthesis process requires the participation of hydroiodic acid. As a strong acid, hydroiodic acid is highly corrosive, and its vapor or smoke is a strong irritant to the eyes, skin, mucous membranes and respiratory tract, and can cause burns to the human body. Therefore, in large-scale industrial production, the large-scale use of hydroiodic acid poses a huge safety hazard.
[0003] However, when sodium iodide or potassium iodide is directly used to synthesize formamidine iodide, the byproduct sodium acetate or potassium acetate has very similar solubility to the product formamidine iodide, making it difficult to separate the product and the byproduct. Therefore, using sodium iodide or potassium iodide, which is cheaper and safer to operate, as an iodine source and solving the problem of separating the byproduct from formamidine iodide is of great significance for the industrial large-scale safe production of formamidine iodide. Summary of the invention
[0004] In view of the above problems, the present invention provides a method for synthesizing formamidine iodide using anion exchange resin as an ion exchange medium to solve the safety hazards of using a large amount of hydroiodic acid and the problem of difficulty in separating the product formamidine iodide and the by-product sodium acetate or potassium acetate in the process of synthesizing formamidine iodide using sodium iodide or potassium iodide.
[0005] To solve the above problems, the technical solution adopted by the present invention consists of the following steps:
[0006] (1) Pretreatment of anion exchange resin
[0007] The factory-produced Cl-type strongly basic anion exchange resin is soaked in a saturated NaCl solution for 1 to 3 days to obtain a saturated Cl-type anion exchange resin, and then the NaCl solution is removed by filtration, and the resin is washed with distilled water to remove the residual NaCl on the surface of the resin to obtain a pretreated Cl-type anion exchange resin.
[0008] (2) Replacement of Cl-type anion exchange resin with I-type
[0009] Add NaI aqueous solution or KI aqueous solution to the pretreated Cl-type anion exchange resin and stir at room temperature for 1 to 3 days; after the replacement is completed, filter out the NaI aqueous solution or KI aqueous solution, wash with distilled water to obtain I-type anion exchange resin. The synthetic route for replacing the anion exchange resin from Cl-type to I-type is:
[0010]
[0011] The main purpose of this step is to replace the anion resin from Cl type to I type. Therefore, in this step, the higher the concentration of NaI or KI aqueous solution, the faster the anion resin is replaced from Cl type to I type, and the shorter the time required for replacement.
[0012] (3) Preparation of formamidine iodide using type I anion exchange resin
[0013] Add an aqueous solution of formamidine acetate to a type I anion exchange resin and stir at room temperature for 1 to 3 days; after the replacement is completed, filter out the insoluble anion exchange resin, and repeat the replacement of the obtained filtrate with a new type I anion exchange resin for 1 to 3 times. Finally, the filtrate obtained after the replacement is dried by a rotary evaporator to dry the solvent, and then vacuum dry to obtain formamidine iodide. The synthetic route for preparing formamidine iodide using type I anion exchange resin is:
[0014]
[0015] In the above synthetic route, ⊕Cl - Represents Cl-type anion exchange resin; ⊕I - Indicates type I anion exchange resin: ⊕CH3COO - Represents CH3COO type anion exchange resin.
[0016] The main purpose of this step is to make the raw material formamidine acetate react fully. Therefore, in this step, the higher the concentration of the formamidine acetate aqueous solution, the slower the speed of completely replacing the formamidine acetate with formamidine iodide, and the longer the time required.
[0017] In the above step (1), the strong basic anion exchange resin is any one of 717 strong basic anion exchange resin, 711 strong basic anion exchange resin, 213 strong basic anion exchange resin, and D202 strong basic anion exchange resin.
[0018] In the above step (2), the concentration of the NaI aqueous solution or the KI aqueous solution is preferably 1 to 5 mol / L.
[0019] In the above step (3), the concentration of the aqueous solution of formamidine acetate is preferably 0.2 to 1 mol / L.
[0020] The beneficial effects of the present invention are as follows:
[0021] The present invention uses NaI or KI as an iodine source and adopts a Cl-type strong alkaline anion exchange resin as an ion exchange medium, thereby realizing the successful synthesis of formamidine iodide. Compared with other methods, the use of low-cost NaI or KI as a raw material not only avoids the potential safety hazards in the process of using HI, but also adopts a common solid-liquid filtration separation method to realize the effective separation of formamidine iodide, solving the problem of difficult separation of formamidine iodide and byproduct sodium acetate or potassium acetate. The preparation method of the present invention is safe and economical, and the synthesized formamidine iodide has high purity and is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is the XRD spectrum of the formamidine iodide synthesized in Example 1.
[0023] Figure 2 This is the IR spectrum of the formamidine iodide synthesized in Example 1.
[0024] Figure 3 The iodine formamidine synthesized in Example 1 1 H NMR spectrum. DETAILED DESCRIPTION
[0025] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments, but the protection scope of the present invention is not limited to these embodiments.
[0026] Example 1
[0027] (1) Pretreatment of anion exchange resin
[0028] Take 120g of 717 strong alkaline anion exchange resin (provided by Fuchen (Tianjin) Chemical Reagent Co., Ltd.) with a factory Cl type, add it to 200mL of saturated NaCl solution and soak it for 3 days to obtain a saturated Cl type anion exchange resin, then remove the NaCl solution by filtration, and wash it with distilled water 3 times to remove the NaCl remaining on the surface of the resin to obtain a pretreated Cl type anion exchange resin.
[0029] (2) Replacement of Cl-type anion exchange resin with I-type
[0030] 100 mL of 1 mol / L NaI aqueous solution was added to the pretreated Cl-type anion exchange resin and stirred at room temperature for 3 days; after the replacement was completed, the NaI aqueous solution was filtered out and washed with distilled water for 3 times to obtain a I-type anion exchange resin.
[0031] (3) Preparation of formamidine iodide using type I anion exchange resin
[0032] Take 40g I type anion exchange resin, add it to 100mL concentration is 0.2mol / L acetate formamidine aqueous solution, stir at room temperature 1 day.After the first displacement ends, filter out the exchange resin that insoluble anion is acetate, add new 40g I type anion exchange resin to the filtrate obtained, and stir at room temperature 1 day.Then filter out the exchange resin that insoluble anion is acetate, complete the second displacement.Finally, add 40g I type anion exchange resin to the filtrate obtained by the second displacement, stir at room temperature 1 day, filter out the exchange resin that insoluble anion is acetate, complete the third displacement.The filtrate obtained after 3 displacements is spin-dried for solvent by rotary evaporator, and finally 70 DEG C of vacuum drying 24h obtains 3.02g iodinated formamidine.
[0033] Depend on Figure 1 and Figure 2 It can be seen that the XRD spectrum and IR spectrum of the formamidine iodide synthesized in this example are consistent with the formamidine iodide with a purity of 99.5% purchased by Anaiji, indicating that the formamidine iodide was successfully synthesized. Figure 3 It can be seen that at 8.66-9.02 ppm, the integrals of 1.99 and 2.02 represent the two hydrogens of -NH2 in formamidine iodide, and at 7.88 ppm, the integral of 1.00 represents the hydrogen of -CH in formamidine iodide. 1 H NMR also confirmed the successful synthesis of formamidine iodide.
[0034] Example 2
[0035] (1) Pretreatment of anion exchange resin
[0036] Take 120g of 717 strong alkaline anion exchange resin of Cl type, add it into 200mL saturated NaCl solution and soak it for 3 days to obtain saturated Cl type anion exchange resin, then remove the NaCl solution by filtration, and wash it with distilled water 3 times to remove the NaCl remaining on the surface of the resin to obtain the pretreated Cl type anion exchange resin.
[0037] (2) Replacement of Cl-type anion exchange resin with I-type
[0038] 100 mL of 3 mol / L NaI aqueous solution was added to the pretreated Cl-type anion exchange resin and stirred at room temperature for 2 days; after the replacement was completed, the NaI aqueous solution was filtered out and washed with distilled water for 3 times to obtain a I-type anion exchange resin.
[0039] (3) Preparation of formamidine iodide using type I anion exchange resin
[0040] Take 40g I type anion exchange resin, add it to 100mL concentration is 0.6mol / L acetic acid formamidine aqueous solution, stir at room temperature for 2 days.After the 1st displacement ends, filter out the exchange resin that insoluble anion is acetate, add new 40g I type anion exchange resin to the filtrate obtained, and stir at room temperature for 2 days.Then filter out the exchange resin that insoluble anion is acetate, complete the 2nd displacement.Finally, add 40g I type anion exchange resin to the filtrate obtained by the 2nd displacement, stir at room temperature for 2 days, filter out the exchange resin that insoluble anion is acetate, complete the 3rd displacement.The filtrate obtained after 3 displacements is spin-dried for solvent by rotary evaporator, and finally 70 DEG C of vacuum drying 24h obtains 8.70g iodinated formamidine.
[0041] Example 3
[0042] (1) Pretreatment of anion exchange resin
[0043] Take 120g of 717 strong alkaline anion exchange resin of Cl type, add it into 200mL saturated NaCl solution and soak it for 3 days to obtain saturated Cl type anion exchange resin, then remove the NaCl solution by filtration, and wash it with distilled water 3 times to remove the NaCl remaining on the surface of the resin to obtain the pretreated Cl type anion exchange resin.
[0044] (2) Replacement of Cl-type anion exchange resin with I-type
[0045] 100 mL of 5 mol / L NaI aqueous solution was added to the pretreated Cl-type anion exchange resin and stirred at room temperature for 1 day. After the replacement was completed, the NaI aqueous solution was filtered out and washed with distilled water for 3 times to obtain a I-type anion exchange resin.
[0046] (3) Preparation of formamidine iodide using type I anion exchange resin
[0047] Take 40g I type anion exchange resin, add it to 100mL concentration is 1mol / L acetic acid formamidine aqueous solution, stir at room temperature for 3 days.After the first displacement ends, filter out the exchange resin that insoluble anion is acetate, add new 40g I type anion exchange resin to the filtrate obtained, and stir at room temperature for 3 days.Then filter out the exchange resin that insoluble anion is acetate, complete the second displacement.Finally, add 40g I type anion exchange resin to the filtrate obtained by the second displacement, stir at room temperature for 3 days, filter out the exchange resin that insoluble anion is acetate, complete the third displacement.The filtrate obtained after 3 displacements is spin-dried for solvent by rotary evaporator, and finally 70 DEG C of vacuum drying 24h obtains 14.22g iodinated formamidine.
[0048] Example 4
[0049] (1) Pretreatment of anion exchange resin
[0050] Take 120g of 717 strong alkaline anion exchange resin of Cl type, add it into 200mL saturated NaCl solution and soak it for 3 days to obtain saturated Cl type anion exchange resin, then remove the NaCl solution by filtration, and wash it with distilled water 3 times to remove the NaCl remaining on the surface of the resin to obtain the pretreated Cl type anion exchange resin.
[0051] (2) Replacement of Cl-type anion exchange resin with I-type
[0052] 100 mL of 5 mol / L KI aqueous solution was added to the pretreated Cl-type anion exchange resin and stirred at room temperature for 1 day. After the replacement was completed, the KI aqueous solution was filtered out and washed with distilled water for 3 times to obtain a I-type anion exchange resin.
[0053] (3) Preparation of formamidine iodide using type I anion exchange resin
[0054] Take 40g I type anion exchange resin, add it to 100mL concentration is 1mol / L acetic acid formamidine aqueous solution, stir at room temperature for 3 days.After the first displacement ends, filter out the exchange resin that insoluble anion is acetate, add new 40g I type anion exchange resin to the filtrate obtained, and stir at room temperature for 3 days.Then filter out the exchange resin that insoluble anion is acetate, complete the second displacement.Finally, add 40g I type anion exchange resin to the filtrate obtained by the second displacement, stir at room temperature for 3 days, filter out the exchange resin that insoluble anion is acetate, complete the third displacement.The filtrate obtained after 3 displacements is spin-dried for solvent by rotary evaporator, and finally 70 DEG C of vacuum drying 24h obtains 13.85g iodinated formamidine.
[0055] The formamidine iodide products obtained in Examples 1 to 4 above were evaluated, and the evaluation results are shown in Table 1.
[0056] Table 1 Yield and purity of the iodinated formamidine products obtained in Examples 1 to 4
[0057] Yield of formamidine iodide (%) Purity of formamidine iodide (%) Example 1 87.8 >99 Example 2 84.3 >99 Example 3 82.7 >99 Example 4 80.5 >99
[0058] As can be seen from Table 1, the yield and purity of the formamidine iodide obtained by the method of the present invention are both high.
Claims
1. A method for synthesizing formamidine iodide using anion exchange resin as an ion exchange medium, characterized in that The method consists of the following steps: (1) Pretreatment of anion exchange resin The factory-produced Cl-type strongly basic anion exchange resin is soaked in a saturated NaCl solution for 1 to 3 days to obtain a saturated Cl-type anion exchange resin, and then the NaCl solution is removed by filtration, and the resin is washed with distilled water to remove the residual NaCl on the surface of the resin to obtain a pretreated Cl-type anion exchange resin; (2) Replacement of Cl-type anion exchange resin with I-type Adding NaI aqueous solution or KI aqueous solution to the pretreated Cl-type anion exchange resin and stirring at room temperature for 1 to 3 days; after the replacement is completed, filtering out the NaI aqueous solution or KI aqueous solution, washing with distilled water to obtain a I-type anion exchange resin; wherein the concentration of the NaI aqueous solution or KI aqueous solution is 1 to 5 mol / L; (3) Preparation of formamidine iodide using type I anion exchange resin An aqueous formamidine acetate solution is added to a type I anion exchange resin and stirred at room temperature for 1 to 3 days; after the replacement is completed, the insoluble anion exchange resin is filtered out, and the obtained filtrate is repeatedly replaced with a new type I anion exchange resin for 1 to 3 times, and finally the filtrate obtained after the replacement is dried by a rotary evaporator to dry the solvent, and then vacuum dried to obtain formamidine iodide; wherein the concentration of the aqueous formamidine acetate solution is 0.2 to 1 mol / L.
2. The method for synthesizing formamidine iodide using anion exchange resin as an ion exchange medium according to claim 1, characterized in that: In step (1), the strong base anion exchange resin is any one of 717 strong base anion exchange resin, 711 strong base anion exchange resin, 213 strong base anion exchange resin, and D202 strong base anion exchange resin.