A low temperature performance enhancer for waterproof asphalt and a preparation method thereof, and waterproof asphalt
The low-temperature performance enhancer prepared by mixing oil components with a specific proportion of mixed heating, solves the problems of low-temperature performance and stability of waterproof asphalt, and achieves the improvement of low-temperature flexibility of asphalt and the stability of softening point and needle inlet.
Patent Information
- Application Number
- CN202310718230.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-06-16
AI Technical Summary
The existing waterproof asphalt has shortcomings in low-temperature performance and stability, especially the volatility of soft components leads to aging resistance and low-temperature performance.
A specific proportion of reduced pressure line oil, furfural extracted oil, mineral oil and aromatic oil mixed with reduced pressure residue oil are used to prepare a low-temperature performance enhancer to improve the low-temperature performance of asphalt and maintain the stability of softening point and needle inlet. sex.
It effectively improves the low temperature flexibility of asphalt to no cracks below -26.0℃, while maintaining the stability of softening points and needle inlet, and improving the overall performance of waterproof asphalt.
Smart Images

Figure BDA0004290128980000011 
Figure BDA0004290128980000031 
Figure BDA0004290128980000071
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of asphalt batching, and in particular to a low-temperature performance enhancer for waterproof asphalt and a preparation method thereof, as well as waterproof asphalt. Background Art
[0002] Asphalt waterproofing membrane is a traditional waterproofing material with advantages such as low cost and easy construction. However, its technical indicators such as tensile strength, stability, and low temperature performance have always been the most concerned in the industry. Asphalt is an extremely complex mixture of hydrocarbons and metal and non-metal derivatives. Due to its excellent hydrophobic and anti-corrosion properties, it is used as the main material for the coating layer of waterproofing membrane. The high and low temperature performance and component composition of asphalt have a crucial impact on the performance of the membrane.
[0003] At present, the waterproof asphalt on the market is mainly obtained by blending road petroleum asphalt with soft components. The advantage is that the waterproof asphalt has better fluidity and is more conducive to the production of waterproof membrane manufacturers; the disadvantage is that the soft component plays a decisive role in the indicators of waterproof asphalt, especially the low-temperature flexibility, softening point and other indicators. Moreover, the soft component is easy to volatilize during the production process of waterproof asphalt, which will lead to the reduction of the anti-aging performance and low-temperature performance of the waterproof membrane. Summary of the invention
[0004] In view of this, the present invention provides a low temperature performance enhancer for waterproof asphalt and a preparation method thereof, as well as waterproof asphalt. The enhancer provided by the present invention can effectively improve the low temperature performance of asphalt and ensure the stability of softening point and needle penetration.
[0005] The present invention provides a low temperature performance enhancer, which comprises the following components in parts by mass:
[0006]
[0007] Preferably, the vacuum line oil is a side-line fraction obtained from the vacuum distillation of petroleum, with a distillation range of 390-450°C and a kinematic viscosity of 60-100 mm at 40°C. 2 / s, wax content ≤5wt%.
[0008] Preferably, the specifications of the furfural extracted oil are: flash point ≥ 230°C, aromatic content ≥ 50wt%, and ash content ≤ 0.5wt%.
[0009] Preferably, the specifications of the mineral oil are: flash point ≥ 230°C, saturated content ≥ 50wt%, and ash content ≤ 0.5wt%.
[0010] Preferably, the mineral oil includes at least one of lubricating oil, hydraulic oil and vacuum pump oil.
[0011] Preferably, the specifications of the aromatic oil are: flash point ≥ 190°C, aromatic hydrocarbon content ≥ 70wt%, and saturated hydrocarbon content ≥ 20wt%.
[0012] Preferably, the specifications of the vacuum residue are: ash content ≤0.5wt%, wax content ≤4wt%, asphaltene content ≥20wt%, colloid content ≥30wt%, saturated content ≤20wt%, and aromatic content ≤30wt%.
[0013] The present invention also provides a method for preparing the low temperature performance enhancer for waterproof asphalt described in the above technical solution, comprising the following steps:
[0014] The vacuum line oil, furfural extracted oil, mineral oil, aromatic oil and vacuum residue oil are mixed and heated to obtain a low temperature performance enhancer for waterproof asphalt.
[0015] Preferably, the method specifically comprises the following steps:
[0016] Add vacuum line oil, furfural extracted oil and mineral oil into the reactor, heat and stir while keeping warm, then add aromatic oil and vacuum residue oil, continue to stir while keeping warm, and after stirring, cool down to obtain a low temperature performance enhancer for waterproof asphalt.
[0017] The present invention also provides a waterproof asphalt, comprising: asphalt and a lifting agent;
[0018] Wherein, the enhancer is the low temperature performance enhancer for waterproof asphalt described in the above technical solution.
[0019] The low-temperature performance enhancer for waterproof asphalt provided by the present invention is prepared by mixing certain vacuum line oil, furfural extracted oil, mineral oil, aromatic oil and vacuum residue oil in a certain proportion, so as to change the component proportion of waterproof asphalt, improve the low-temperature performance of asphalt, and ensure the stability of softening point and needle penetration without causing adverse effects on the softening point and needle penetration.
[0020] The test results show that the low-temperature performance enhancer provided by the present invention can make the low-temperature flexibility of asphalt reach no cracks below -26.0°C, effectively improving its low-temperature flexibility. At the same time, its softening point and needle penetration do not change significantly, ensuring the stability of the softening point and needle penetration. DETAILED DESCRIPTION
[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0022] In this article, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0023] Herein, when it comes to numerical ranges, unless otherwise specified, the numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0024] In this article, when referring to the unit of a data range, if there is a unit only after the right endpoint, it means that the units of the left and right endpoints are the same. For example, 0.3-0.5m / s means that the units of the left endpoint "0.3" and the right endpoint "0.5" are both m / s (meters per second).
[0025] Only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and likewise any upper limit can be combined with any other upper limit to form an unspecified range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an unspecified range.
[0026] The present invention provides a low temperature performance enhancer for waterproof asphalt, which comprises the following components in parts by mass:
[0027]
[0028] About decompression line oil:
[0029] In the present invention, the vacuum line oil is a side-line fraction obtained from the vacuum distillation of petroleum. In the present invention, the specifications of the vacuum line oil are preferably: a distillation range of 390 to 450°C, a kinematic viscosity of 60 to 100 mm at 40°C 2 / s, wax content ≤5wt%. The kinematic viscosity at 40°C may be 60mm 2 / s, 65mm 2 / s, 70mm 2 / s, 75mm 2 / s, 80mm 2 / s, 85mm 2 / s, 90mm 2 / s, 95mm 2 / s、100mm2 / s. The wax content can be 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%. In some embodiments of the present invention, the specification of the vacuum line oil is: the distillation range is 390-450℃, the kinematic viscosity at 40℃ is 70mm 2 / s, wax content 4.5wt%.
[0030] In the present invention, the content of the vacuum line oil is 50 to 80 parts, specifically 50 parts, 51 parts, 52 parts, 53 parts, 54 parts, 55 parts, 56 parts, 57 parts, 58 parts, 59 parts, 60 parts, 61 parts, 62 parts, 63 parts, 64 parts, 65 parts, 66 parts, 67 parts, 68 parts, 69 parts, 70 parts, 71 parts, 72 parts, 73 parts, 74 parts, 75 parts, 76 parts, 77 parts, 78 parts, 79 parts, and 80 parts.
[0031] About furfural extracted oil:
[0032] The furfural extracted oil refers to the non-ideal components of lubricating oil separated from the vacuum distillate oil or solvent deasphalted oil by furfural solvent extraction, dissolved in the furfural solvent. In the present invention, the specifications of the furfural extracted oil are preferably: flash point ≥ 230°C, aromatic content ≥ 50wt%, ash content ≤ 0.5wt%. Among them, the flash point can be specifically 230°C, 235°C, 240°C, etc. The aromatic content can be specifically 50wt%, 51wt%, 52wt%, 53wt%, 54wt%, 55wt%, 60wt%, etc. The ash content can be specifically 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%. In some embodiments of the present invention, the specifications of the furfural extracted oil are: flash point 240°C, aromatic content 55wt%, ash content 0.3wt%.
[0033] In the present invention, the content of the furfural extracted oil is 1 to 5 parts, specifically 1 part, 2 parts, 3 parts, 4 parts, and 5 parts.
[0034] About mineral oil:
[0035] In the present invention, the mineral oil preferably includes at least one of lubricating oil, hydraulic oil and vacuum pump oil. The lubricating oil is a mechanical lubricating oil, preferably including engine oil and / or non-engine oil lubricating oil. In the present invention, the specifications of the mineral oil are preferably: flash point ≥ 230°C, saturated content ≥ 50wt%, ash content ≤ 0.5wt%. Wherein, the flash point can be specifically 230°C, 235°C, 240°C, etc. The saturated content can be specifically 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, 75wt%, 80wt%, etc. The ash content can be specifically 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%. In some embodiments of the present invention, the specifications of the mineral oil are: flash point 230°C, saturated content 80wt%, ash content 0.1wt%.
[0036] In the present invention, the content of the mineral oil is 5 to 20 parts, specifically 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, and 20 parts.
[0037] About aromatic oil:
[0038] Aromatic oil is also called aromatic oil. In the present invention, the specifications of the aromatic oil are preferably: flash point ≥ 190°C, distillation range 220-400°C, aromatic hydrocarbon content ≥ 70wt%, saturated hydrocarbon proportion ≥ 20wt%. Wherein, the flash point can be specifically 190°C, 200°C, 210°C, 220°C, 230°C. The aromatic hydrocarbon content can be specifically 70wt%, 75wt%, etc. The saturated hydrocarbon proportion can be specifically 20wt%, 25wt%, etc. In some embodiments of the present invention, the specifications of the aromatic oil are preferably: flash point 200°C, distillation range 220-400°C, aromatic hydrocarbon content 70wt%, saturated hydrocarbon content 20wt%.
[0039] In the present invention, the content of the aromatic oil is 5 to 20 parts, specifically 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, and 20 parts.
[0040] About vacuum residue:
[0041] Vacuum residue (also known as vacuum distillation residue) refers to the residual oil extracted from the bottom of the vacuum tower of the refinery, which is the heaviest component remaining after the crude oil is distilled under vacuum. The chemical composition of vacuum residue is often analyzed by separating vacuum residue into saturated fractions, aromatic fractions, colloids and asphaltenes, that is, the chemical composition of vacuum residue is expressed by the proportion of the above four components. In the present invention, the specifications of the vacuum residue are preferably: ash content ≤0.5wt%, wax content ≤4wt%, asphaltene content ≥20wt%, colloid content ≥30wt%, saturated fraction content ≤20wt%, aromatic fraction content ≤30wt%. Among them, the ash content can be specifically 0.10wt%, 0.15wt%, 0.20wt%, 0.25wt%, 0.30wt%, 0.35wt%, 0.40wt%, 0.45wt%, 0.50wt%. The wax content can be specifically 1wt%, 2wt%, 3wt%, 4wt%. The asphaltene content can be 20wt%, 25wt%, 30wt%, 33wt%, 35wt%, etc. The gum content can be 30wt%, 35wt%, etc. The saturated content can be 5wt%, 7wt%, 10wt%, 15wt%, 20wt%. The aromatic content can be 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%. In some embodiments of the present invention, the specifications of the vacuum residue are: ash content 0.45wt%, wax content 4wt%, asphaltene content 33wt%, gum content 35wt%, saturated content 7wt%, aromatic content 25wt%.
[0042] In the present invention, the content of the vacuum residue is 5 to 20 parts, specifically 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, and 20 parts.
[0043] In some embodiments of the present invention, the raw material composition of the lifting agent is: 80 parts of vacuum line oil, 3 parts of furfural extracted oil, 7 parts of mineral oil, 5 parts of aromatic oil, and 5 parts of vacuum residue oil. In other embodiments of the present invention, the raw material composition of the lifting agent is: 70 parts of vacuum line oil, 1 part of furfural extracted oil, 14 parts of mineral oil, 10 parts of aromatic oil, and 5 parts of vacuum residue oil. In other embodiments of the present invention, the raw material composition of the lifting agent is: 50 parts of vacuum line oil, 5 parts of furfural extracted oil, 20 parts of mineral oil, 20 parts of aromatic oil, and 20 parts of vacuum residue oil.
[0044] In some embodiments of the present invention, the type and specifications of the lifting agent raw materials are as follows: vacuum line oil: 40°C kinematic viscosity 70mm 2 / s, wax content 4.5wt%, distillation range 390~450℃. Furfural extracted oil: flash point 240℃, aromatic content 55wt%, ash content 0.3wt%. Mineral oil: flash point 230℃, saturated content 80wt%, ash content 0.1wt%. Aromatic oil: flash point 200℃, aromatic content 70wt%, saturated content 20wt%, distillation range 220~400℃. Vacuum residue: ash content 0.45wt%, wax content 4wt%, asphaltene content 33wt%, colloid content 35wt%, saturated content 7wt%, aromatic content 25wt%.
[0045] The present invention also provides a method for preparing the low-temperature performance enhancer for waterproof asphalt described in the above technical scheme, comprising the following steps: mixing and heating vacuum line oil, furfural extracted oil, mineral oil, aromatic oil and vacuum residue oil to obtain the low-temperature performance enhancer for waterproof asphalt.
[0046] In the present invention, the above-mentioned preparation method preferably specifically comprises: adding vacuum line oil, furfural extraction oil and mineral oil to the reactor, heating and heat preservation and stirring, then adding aromatic oil and vacuum residue oil, continuing to heat preservation and stirring, and cooling after the stirring is completed to obtain a low-temperature performance enhancer for waterproof asphalt. Among them, the target temperature of the heating is preferably 80-100°C, specifically 80°C, 85°C, 90°C, 95°C, 100°C. The time for heat preservation and stirring after heating to the above-mentioned target temperature is preferably 20-30min, specifically 20min, 25min, 30min. After adding aromatic oil and vacuum residue oil, the time for heat preservation and stirring is preferably 20-30min, specifically 20min, 25min, 30min. After the stirring is completed, it is cooled to room temperature to obtain a low-temperature performance enhancer for waterproof asphalt.
[0047] The present invention also provides a waterproof asphalt, comprising: asphalt and an enhancer; wherein the enhancer is the low-temperature performance enhancer for waterproof asphalt described in the above technical solution.
[0048] In the present invention, the type of the asphalt is not particularly limited, and it can be conventional asphalt in the art. In the present invention, the amount of the enhancer is preferably 43% to 81% of the mass of the asphalt, specifically 43%, 50%, 55%, 60%, 67%, 70%, 75%, 80%, 81%.
[0049] The low-temperature performance enhancer for waterproof asphalt provided by the present invention is prepared by mixing certain vacuum line oil, furfural extracted oil, mineral oil, aromatic oil and vacuum residue oil in a certain proportion, so as to change the component proportion of waterproof asphalt, improve the low-temperature performance of asphalt, and ensure the stability of softening point and needle penetration without causing adverse effects on the softening point and needle penetration.
[0050] The test results show that the low-temperature performance enhancer provided by the present invention can make the low-temperature flexibility of asphalt reach no cracks below -26.0°C, effectively improving its low-temperature flexibility. At the same time, its softening point and needle penetration do not change significantly, ensuring the stability of the softening point and needle penetration.
[0051] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0052] Example 1
[0053] 1. Raw materials:
[0054]
[0055] The specifications of each raw material are shown in Table 1:
[0056] Table 1: Types of raw materials in Example 1
[0057]
[0058] 2. Preparation:
[0059] Add vacuum line oil, furfural extracted oil and mineral oil into the reactor, heat to 80°C, keep warm and stir for 30 minutes, then add aromatic oil and vacuum residue oil in turn, continue to keep warm and stir for 30 minutes, after stirring, cool to room temperature to obtain the enhancer.
[0060] Example 2
[0061] 1. Raw materials:
[0062]
[0063]
[0064] The specifications of the raw materials are the same as those in Table 1 of Example 1.
[0065] 2. Preparation:
[0066] Add vacuum line oil, furfural extracted oil and mineral oil into the reactor, heat to 80°C, keep warm and stir for 30 minutes, then add aromatic oil and vacuum residue oil in turn, continue to keep warm and stir for 30 minutes, after stirring, cool to room temperature to obtain the enhancer.
[0067] Example 3
[0068] 1. Raw materials:
[0069]
[0070] The specifications of the raw materials are the same as those in Table 1 of Example 1.
[0071] 2. Preparation:
[0072] Add vacuum line oil, furfural extracted oil and mineral oil into the reactor, heat to 80°C, keep warm and stir for 30 minutes, then add aromatic oil and vacuum residue oil in turn, continue to keep warm and stir for 30 minutes, after stirring, cool to room temperature to obtain the enhancer.
[0073] Comparative Example 1
[0074] Vacuum line oil (same type as in Example 1) was used as a lifting agent.
[0075] Comparative Example 2
[0076] The implementation is carried out according to Example 1, except that the distribution ratio of each group in the raw material is adjusted as follows:
[0077]
[0078] Comparative Example 3
[0079] The implementation is carried out according to Example 1, except that the distribution ratio of each group in the raw material is adjusted as follows:
[0080]
[0081] Comparative Example 4
[0082] The process was carried out in accordance with Example 1, except that furfural extracted oil and mineral oil were not added to the raw materials.
[0083] Comparative Example 5
[0084] The process was carried out in accordance with Example 1, except that aromatic oil and vacuum residue oil were not added to the raw materials.
[0085] Test example:
[0086] The enhancer and 70# asphalt were mixed in a mass ratio of 4:6, heated to 100°C, and stirred for 60 minutes to obtain waterproof asphalt.
[0087] The softening point, penetration and low temperature flexibility of the obtained waterproof asphalt were tested. The softening point test was in accordance with T0606-2011, the penetration test was in accordance with T0604-2011, and the low temperature flexibility test was in accordance with GB / T328.14-2016. The test results are shown in Table 4.
[0088] Table 4: Test results
[0089]
[0090] It can be seen from the test results in Table 4 that, compared with Comparative Example 1, the low-temperature flexibility of Examples 1-3 of the present invention is improved by more than 1.5°C, while the softening point and needle penetration are basically the same. This shows that the enhancer of the present invention can significantly improve the low-temperature performance of waterproof asphalt and ensure the stability of the softening point and needle penetration indicators.
[0091] Compared with the embodiment, although the low-temperature flexibility of Comparative Example 2 is improved, the change range of the softening point and needle penetration is increased, and the technical indicators do not meet the standards; compared with the embodiment, the low-temperature flexibility of Comparative Example 3 is decreased, and the change range of the softening point and needle penetration is increased, and the technical indicators do not meet the standards; it proves that the raw materials of the present invention are matched in a certain proportion to effectively improve the low-temperature performance of asphalt and ensure the stability of the softening point and needle penetration indicators. Compared with the embodiment, the low-temperature flexibility of Comparative Example 4 is decreased, and the change range of the softening point and needle penetration is increased; compared with the embodiment, although the low-temperature flexibility of Comparative Example 5 is basically the same, the change range of the softening point and needle penetration is increased; it proves that the present invention combines the above 5 raw materials together to effectively improve the low-temperature performance of asphalt and ensure the stability of the softening point and needle penetration indicators.
[0092] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enable any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.
Claims
1. A waterproof asphalt, characterized in that: include: 70# asphalt and low temperature performance enhancer for waterproof asphalt; The dosage of the enhancer is 43% to 81% of the asphalt mass; Wherein, the low temperature performance enhancer for waterproof asphalt comprises the following components in parts by mass: The vacuum line oil is a side-line fraction obtained from the vacuum distillation of petroleum, with a distillation range of 390-450°C and a kinematic viscosity of 70 mm at 40°C. 2 / s, wax content 4.5wt%; The specifications of the furfural extracted oil are: flash point 240°C, aromatic content 55wt%, ash content 0.3wt%; The specifications of the mineral oil are: flash point 230°C, saturated content 80wt%, ash content 0.1wt%; The specifications of the aromatic oil are: flash point 200°C, aromatic hydrocarbon content 70wt%, saturated hydrocarbon content 20wt%, distillation range 220-400°C; The specifications of the vacuum residue are: ash content 0.45wt%, wax content 4wt%, asphaltene content 33wt%, colloid content 35wt%, saturated content 7wt%, aromatic content 25wt%; The mineral oil includes at least one of lubricating oil, hydraulic oil and vacuum pump oil.
2. The waterproof asphalt according to claim 1, characterized in that: The method for preparing the low temperature performance enhancer for waterproof asphalt comprises the following steps: The vacuum line oil, furfural extracted oil, mineral oil, aromatic oil and vacuum residue oil are mixed and heated to obtain a low temperature performance enhancer for waterproof asphalt.
3. The waterproof asphalt according to claim 2, characterized in that: The specific steps include: Add vacuum line oil, furfural extracted oil and mineral oil into the reactor, heat and stir while keeping warm, then add aromatic oil and vacuum residue oil, continue to stir while keeping warm, and after stirring, cool down to obtain a low temperature performance enhancer for waterproof asphalt.