High-voltage lithium ion battery electrolyte and lithium ion battery thereof

By using polyether modified polysiloxane as an electrolyte additive in lithium-ion batteries, the problems of electrolyte decomposition and silicon carbon negative electrode expansion are solved, and the high-temperature fast charging, low-temperature and rate performance of lithium-ion batteries are improved, and the high-temperature fast charging, low-temperature and magnification performance of lithium-ion batteries are achieved. Longer battery life and more stable battery performance.

CN119029311APending Publication Date: 2024-11-26ZHUHAI SMOOTHWAY ELECTRONICS MATERIALS
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411324559.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing lithium-ion batteries have problems such as electrolyte decomposition, silicon carbon negative electrode expansion and performance deterioration under high voltage conditions, making it difficult to meet the needs of high energy density and long cycle life.

Method used

Polyether modified polysiloxane is used as an additive for non-aqueous electrolyte to reduce the viscosity of the electrolyte, increase the transmission speed of lithium ions, and does not decompose significantly under high voltage. Partially deposited at the interface of silicon-carbon negative electrode to alleviate expansion Pressure inhibits the decomposition of electrolyte solvents and improves the battery's high-temperature fast charging, low-temperature and rate performance.

Benefits of technology

It significantly improves the high-temperature fast charging cycle performance, low-temperature performance and rate performance of lithium-ion batteries, maintains a stable SEI film, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005055043630000041
    Figure BDA0005055043630000041
  • Figure BDA0005055043630000051
    Figure BDA0005055043630000051
  • Figure BDA0005055043630000071
    Figure BDA0005055043630000071
Patent Text Reader

Abstract

The invention provides a high-voltage lithium ion battery electrolyte and a lithium ion battery thereof. The high-voltage lithium ion battery electrolyte comprises an electrolyte salt, a non-aqueous organic solvent and an additive, wherein the additive comprises polyether modified polysiloxane. The polyether modified polysiloxane is added into the electrolyte, so that the high-temperature quick-charge cycle performance, the low-temperature performance and the rate capability of the lithium ion battery under high voltage (4.53 V) can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a high-voltage lithium ion battery electrolyte and a lithium ion battery thereof. Background Art

[0002] Consumer products have always been with people's daily life. Among them, lithium-ion batteries, the core power components of consumer batteries, have attracted the attention of the world. Lithium cobalt oxide batteries have been favored by digital batteries because of their high mass energy. As an important component of the battery, the electrolyte plays a decisive role in the performance of the battery. Therefore, it is very necessary to optimize the electrolyte to improve the performance of the battery. The current market development direction is high energy density and long cycle life lithium-ion batteries, which also brings many challenges to the development of electrolytes. For example, under deep lithium deintercalation potential, the catalytic substances (singlet oxygen, transition metals, etc.) released by the positive electrode material shuttle between the positive and negative electrodes, causing the electrolyte solvent to be decomposed and deteriorating the battery performance. The negative electrode development material is moving towards the use of silicon-carbon materials. The volume expansion of silicon-carbon materials brings about problems such as decomposition and gas production of the electrolyte. In order to improve the above problems, it is urgent to develop a high-voltage lithium-ion battery electrolyte and its lithium-ion battery to meet the needs of consumer battery development. Summary of the invention

[0003] The object of the present invention is to provide a high-voltage lithium-ion battery electrolyte and a lithium-ion battery thereof. The non-aqueous electrolyte contains polyether-modified polysiloxane, which can inhibit the decomposition of the non-aqueous electrolyte and can be partially deposited on the surface of the positive and negative electrodes, thereby improving the high-temperature fast-charging cycle performance, low-temperature performance and rate performance of the lithium-ion battery under high voltage (4.53V).

[0004] To achieve the above objectives, the present invention provides a high-voltage lithium-ion battery electrolyte and a lithium-ion battery thereof, comprising an electrolyte salt, a non-aqueous organic solvent and an additive, wherein the additive comprises a polyether-modified polysiloxane.

[0005] Compared with the prior art, the present invention introduces polyether-modified polysiloxane as an additive in the non-aqueous electrolyte, which can reduce the viscosity of the electrolyte as a whole and increase the transmission speed of lithium ions at the electrolyte interface, thereby contributing to the performance of fast charging. The methylsilyl functional group contained in the polyether-modified polysiloxane material can combine with the hydrofluoric acid in the electrolyte to reduce the etching effect of the acidic substance on the interface components, thereby improving the overall interface stability. The advantage of polyether-modified polysiloxane compared with other methylsilyl compounds is that it can not undergo obvious decomposition reaction under high voltage conditions. At the same time, as a polymer itself, it can be partially deposited at the interface of the silicon-carbon negative electrode, which can relieve the stress of the silicon-carbon negative electrode expansion. This mode of action not only improves the stability of the silicon-carbon negative electrode interface, but also inhibits the polymer formed by the decomposition of the electrolyte solvent, which can improve the high-temperature fast charging cycle performance of the battery with high-voltage lithium cobalt oxide matching the silicon-carbon negative electrode, and can also significantly improve the low temperature and rate characteristics. Therefore, the non-aqueous electrolyte can maintain a stable SEI film under long-term cycling conditions, inhibit the oxidative decomposition of the non-aqueous electrolyte, and thereby improve the high-temperature fast-charging cycle performance, low-temperature performance, and rate performance of the lithium-ion battery.

[0006] Preferably, the polyether-modified polysiloxane of the present invention is at least one selected from HY-6085, HY-6086, HY-037, HY-5030, HY-5057, BYK-3560, BYK-3565 and BYK-333.

[0007] Preferably, the polyether-modified polysiloxane of the present invention accounts for 0.05% to 2.0% of the sum of the mass of the non-aqueous organic solvent, the electrolyte salt and the additive. As an example, the polyether-modified polysiloxane accounts for 0.05%, 0.1%, 0.2%, 0.4%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0% of the sum of the mass of the non-aqueous organic solvent, the electrolyte salt and the additive, but is not limited to the listed values, and other values ​​not listed within the above numerical ranges are also applicable.

[0008] Preferably, the electrolyte salt of the present invention is selected from at least one of lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium trifluoromethanesulfonate (LiCF3SO3), lithium bistrifluoromethylsulfonyl imide (LiN(CF3SO2)2), lithium bis(oxalatoborate) (C4BLiO8), lithium difluorophosphate (LiPO2F2), lithium difluorooxalatoborate (C2BF2LiO4), lithium difluorobis(oxalatophosphate) (LiDFBP) and lithium bis(fluorosulfonyl imide) (LiFSI).

[0009] Preferably, the electrolyte salt of the present invention accounts for 5% to 20% of the sum of the mass of the non-aqueous organic solvent, the electrolyte salt and the additive. As an example, the electrolyte salt accounts for 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20% of the sum of the mass of the non-aqueous organic solvent, the electrolyte salt and the additive, but is not limited to the listed values, and other values ​​not listed within the above numerical ranges are also applicable.

[0010] Preferably, the non-aqueous organic solvent of the present invention is selected from at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), pentylene carbonate, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propylene carbonate (PC), butyl acetate (n-Ba), γ-butyrolactone (γ-Bt), propyl propionate (n-PP), ethyl propionate (EP) and ethyl butyrate (Eb), ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, 1,3-dioxolane (DOL), tetrahydrofuran (THF), methyltetrahydrofuran, diphenyl ether and crown ether.

[0011] Preferably, the additive also includes a film-forming aid, which is selected from at least one of vinylene carbonate (VC), vinyl ethylene carbonate (VEC), fluoroethylene carbonate (FEC), vinyl sulfite (ES), 1,3-propane sultone (PS), diethylene sulfate (DTD), adiponitrile (ADN), succinonitrile, 1.3.6-hexanetrinitrile (HTCN), ether trinitrile (CAS: 2465-93-2) and phosphazene.

[0012] Preferably, the film-forming aid of the present invention accounts for 0.05% to 2.0% of the sum of the mass of the non-aqueous organic solvent, the electrolyte salt and the additive. As an example, the film-forming aid accounts for 0.05%, 0.1%, 0.2%, 0.4%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0% of the sum of the mass of the non-aqueous organic solvent, the electrolyte salt and the additive, but is not limited to the listed values, and other values ​​not listed within the above numerical ranges are also applicable.

[0013] Another aspect of the present invention provides a lithium ion battery, comprising a positive electrode material and a negative electrode material, and also comprising the above-mentioned high voltage lithium ion battery electrolyte, and the maximum charging voltage is 4.53V.

[0014] Preferably, the positive electrode material is selected from lithium cobalt oxide.

[0015] Preferably, the negative electrode material is selected from silicon-carbon negative electrode material. DETAILED DESCRIPTION

[0016] In order to better illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be noted that the following implementation method is a further explanation of the present invention and should not be used as a limitation of the present invention.

[0017] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0018] Example 1

[0019] (1) Preparation of non-aqueous electrolyte: In a glove box filled with nitrogen (O2 <2ppm, H2O <3ppm), ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and propyl propionate (PP) were mixed in a weight ratio of EC:DEC:EMC:PP=2:2:1:2 to obtain 85.5g of an organic solvent, and then 0.5g of HY-6085 was added, dissolved, and stirred thoroughly, and then 14g of lithium hexafluorophosphate (LiPF6) was added and mixed uniformly to obtain a non-aqueous electrolyte.

[0020] (2) Preparation of positive electrode: Lithium cobalt oxide (LiCoO2), binder PVDF and conductive agent SuperP are mixed in a mass ratio of 97:1:2 to form a lithium-ion battery positive electrode slurry with a certain viscosity. The mixed slurry is coated on both sides of an aluminum foil, dried and rolled to obtain a positive electrode sheet.

[0021] (3) Preparation of negative electrode: Silicon-carbon negative electrode material (10 wt.% Si) is mixed with conductive agent SuperP, thickener CMC, and adhesive SBR (styrene-butadiene rubber latex) in a mass ratio of 96:1:1:2 to make a slurry, mix them evenly, apply the mixed slurry on both sides of the copper foil, dry and roll-press to obtain the negative electrode sheet.

[0022] (4) Preparation of lithium-ion batteries: The positive electrode sheets, separators and negative electrode sheets are stacked to form a square battery cell, which is packaged with a polymer and filled with the above-prepared lithium-ion battery non-aqueous electrolyte. After the steps of formation and capacity separation, a lithium-ion battery with a capacity of 1400 mAh is manufactured.

[0023] The non-aqueous electrolyte formulations of Examples 1-22 and Comparative Examples 1-4 are shown in Table 1. The steps of preparing the electrolyte and making the battery in Examples 2-22 and Comparative Examples 1-4 are the same as those in Example 1.

[0024] Table 1 Electrolyte components of various embodiments and comparative examples

[0025]

[0026]

[0027] The high temperature fast charge cycle performance, low temperature discharge performance and rate performance tests were performed on the lithium ion batteries prepared in Examples 1 to 22 and Comparative Examples 1 to 4, respectively. The specific test conditions are as follows, and the test results are shown in Table 2.

[0028] (1) High temperature fast charging cycle performance

[0029] Place the lithium-ion battery in a 45℃ constant temperature box and let it stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature. Charge at a constant current of 3C to a voltage of 4.53V, then charge at a constant voltage of 4.53V to a current of 0.05C, then discharge at a constant current of 1C to a voltage of 3.0V, and record the first cycle discharge capacity of the battery as C0. This is one charge and discharge cycle. Then, charge and discharge at 3C / 1C for 300 cycles at 45℃, and record the discharge capacity as C1.

[0030] Capacity retention rate = C1 / C0*100%

[0031] (2) Rate performance test

[0032] At 25°C, charge the formed battery to 4.53V with 1C constant current and constant voltage, then discharge to 3.0V with 0.5C constant current, and record the discharge capacity. Then charge to 4.53V with 1C constant current and constant voltage, then discharge to 3.0V with 1C constant current, and record the discharge capacity; then charge to 4.53V with 1C constant current and constant voltage, then discharge to 3.0V with 2C constant current, and record the discharge capacity. Test the capacity retention rate at different discharge rates. The calculation formula is as follows:

[0033] Capacity retention rate = discharge capacity at different rates / initial capacity × 100%

[0034] (3) Low temperature discharge test

[0035] At room temperature (25°C), the lithium-ion battery is charged and discharged at 0.5C / 0.5C (battery cut-off voltage is 3.0V, discharge capacity is C0), and the upper voltage is 4.53V (cut-off current 0.05C). Then the battery is fully charged to 4.45V (cut-off current 0.05C) at 0.5C at room temperature (25°C), and then the battery is transferred to -20°C and left for 4 hours, and discharged to 3.0V at 0.5C, and the discharge capacity is C1. The capacity retention rate is calculated using the following formula:

[0036] Capacity retention rate = (C1 / C0)*100%

[0037] (4) High temperature cycle gas production test

[0038] The battery was fully charged to 4.53V (cut-off current 0.05C) at room temperature (25°C) at 0.5C, and the battery thickness D1 was tested. Then the fully charged battery was charged and discharged at 1.0C / 1.0C at 45°C for 400 cycles, and the battery thickness D2 was tested. The expansion rate of high-temperature cyclic gas generation was calculated.

[0039] Expansion rate = (D2-D1) / D1*100%

[0040] Table 2 Lithium-ion battery performance test results

[0041]

[0042] It can be seen from the results in Table 2 that based on Comparative Examples 1 to 4, the non-aqueous electrolytes of Examples 1 to 22 of the present invention contain polyether-modified polysiloxane, which can improve the high-temperature storage, -20°C low-temperature discharge performance and rate performance of the lithium cobalt oxide positive electrode material system battery under high voltage (4.53V).

[0043] From the comparison of Examples 1 to 8, it can be seen that when the polyether-modified polysiloxane is HY-6086, its performance is the best, which may be because the number of trimethylsilyl groups at the tail end is greater than that of the others, resulting in excellent overall performance.

[0044] From the comparison between Example 2 and Examples 15 to 22, it can be seen that adding a film-forming aid on the basis of polyether-modified polysiloxane can further improve the electrochemical performance. Among them, from the comparison between Example 2 and Examples 15 to 20, it can be seen that when HY-6086 is used in combination with FEC, the performance improvement is most obvious, which may be because HY-6086 can delay the decomposition of FEC, thereby improving the overall battery cycle performance.

[0045] By comparing Example 1 with Comparative Examples 3 to 4, it can be seen that when the mass of polyether-modified polysiloxane is lower than the range of this application, its fast charging, rate and low-temperature performance are poor. This may be because the low content has little effect on the viscosity of the overall electrolyte and cannot improve the fast charging cycle, rate and low-temperature cycle performance of the battery; when the mass of polyether-modified polysiloxane exceeds the range of this application, its performance is poor. This may be because the added content is too high, which causes the overall electrolyte viscosity to increase, resulting in worse ion kinetics, and thus a decrease in overall electrochemical performance.

[0046] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A high voltage lithium ion battery electrolyte, comprising an electrolyte salt, a non-aqueous organic solvent and an additive, characterized in that: The additive includes polyether-modified polysiloxane.

2. The high voltage lithium ion battery electrolyte according to claim 1, characterized in that: The polyether-modified polysiloxane is selected from at least one of HY-6085, HY-6086, HY-037, HY-5030, HY-5057, BYK-3560, BYK-3565 and BYK-333.

3. The high voltage lithium ion battery electrolyte according to claim 1, characterized in that: The polyether-modified polysiloxane accounts for 0.05% to 2.0% of the total mass of the non-aqueous organic solvent, the electrolyte salt and the additive.

4. The high voltage lithium ion battery electrolyte according to claim 1, characterized in that: The electrolyte salt is selected from at least one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium trifluoromethanesulfonate, lithium bistrifluoromethanesulfonyl imide, lithium bisoxalatoborate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium difluorobisoxalatophosphate and lithium bisfluorosulfonyl imide.

5. The high voltage lithium ion battery electrolyte according to claim 1, characterized in that: The electrolyte salt accounts for 5% to 20% of the total mass of the non-aqueous organic solvent, the electrolyte salt and the additive.

6. The high voltage lithium ion battery electrolyte according to claim 1, characterized in that: The non-aqueous organic solvent is selected from at least one of ethylene carbonate, propylene carbonate, butylene carbonate, pentylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, propylene carbonate, butyl acetate, γ-butyrolactone, propyl propionate, ethyl propionate and ethyl butyrate, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, 1,3-dioxolane, tetrahydrofuran, methyltetrahydrofuran, diphenyl ether and crown ether.

7. The high voltage lithium ion battery electrolyte according to claim 1, characterized in that: The additives also include a film-forming aid, which is selected from at least one of vinylene carbonate, vinyl ethylene carbonate, fluoroethylene carbonate, vinyl sulfite, 1,3-propane sultone, vinyl sulfate, adiponitrile, succinonitrile, 1.3.6-hexane trinitrile, ether trinitrile and phosphazene.

8. The high voltage lithium ion battery electrolyte according to claim 7, characterized in that: The film-forming aid accounts for 0.05% to 2.0% of the total mass of the non-aqueous organic solvent, the electrolyte salt and the additive.

9. A lithium ion battery comprising a positive electrode material and a negative electrode material, characterized in that: It also includes the high-voltage lithium-ion battery electrolyte according to any one of claims 1 to 8, and the maximum charging voltage is 4.53V.

10. The lithium ion battery according to claim 9, characterized in that: The positive electrode material is selected from lithium cobalt oxide.

Citation Information

Cited By

  • Modified polymethylhydrosiloxane electrolyte additive, preparation method, electrolyte and application