A catalyst grading and filling method for hydrogenation of easily coking oil products

By using a catalyst gradation loading method, the main catalyst is isolated by an auxiliary catalyst with a larger porosity, which solves the problem of catalyst adhesion in the hydrorefining process of tar-prone products, and realizes convenient and safe unloading.

CN116554918BActive Publication Date: 2024-11-08CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210110933.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-29
Publication Date
2024-11-08
Estimated Expiration
2042-01-29

AI Technical Summary

Technical Problem

In existing technologies, catalysts in easily tarred oils tend to stick together during hydrorefining, leading to difficulties in unloading, increased labor intensity and safety risks, and vacuum suction methods are difficult to effectively unload dense coke.

Method used

A catalyst gradation loading method is adopted, in which a gradation loading section is set in the reactor inlet section. The auxiliary catalyst with a larger porosity is used to isolate the main catalyst and form a grid distribution. Hollow or toothed particles are filled in the auxiliary area, and porous particles are filled in the main area to reduce catalyst adhesion.

Benefits of technology

It reduces the labor intensity and safety risks of unloading, reduces the maintenance costs of hydrogenation units, and achieves efficient hydrogenation treatment of easily tar-forming oil products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116554918B_ABST
    Figure CN116554918B_ABST
Patent Text Reader

Abstract

A catalyst grading and filling method for hydrogenation of oil products prone to coking is to set a grading and filling section at the inlet section of the reactor, divide the space of the grading and filling section into several main areas and auxiliary areas that isolate the main areas, the auxiliary areas extend axially along the logistics direction in the reactor but do not extend to the end of the reactor, the voidage of the auxiliary areas is 0.40-0.80, and the voidage of the main areas is smaller than the voidage of the auxiliary areas. In the technical solution of the present invention, a catalyst with a lower voidage is filled in the main area, the contact between the catalyst particles is closer, and the strength of the block formed by coking is higher, and an auxiliary area is set between the main areas, and a catalyst with a higher voidage is filled therein, the contact surface between the catalyst particles is smaller, and the strength of the block formed by coking is lower. When it is necessary to unload the coked catalyst, the auxiliary area with lower strength is first broken with tools such as a pneumatic pick, the main area is separated, and the catalyst is unloaded in a more relaxed manner.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oil hydrogenation, and in particular to a catalyst grading and filling method for hydrogenation of oil products prone to coking. Background Art

[0002] Due to the influence of impurities, many oil products need to be hydrogenated to improve their quality before they can be used. For example, ethylene cracking gasoline, coking naphtha, catalytic gasoline, Fischer-Tropsch synthetic oil, coking diesel, catalytic diesel, high-dry point straight-run diesel, wax oil, residual oil, coal tar, coal hydrogenation oil, etc., mostly contain impurities such as sulfur, nitrogen, oxygen, olefins, and aromatics, and usually require hydrogenation and refining to remove the impurities before they can be used. During the hydrorefining process, coking substances in oil products such as olefins and aromatics are easily dehydrogenated and condensed when heated, which sticks the catalyst particles together and makes them difficult to unload. For example, hydrogenation of coking gasoline causes coking on the top of the hydrorefining reactor, and it is very difficult to unload the catalyst at the end of the operation. The large cake-like coked catalyst on the top needs to be broken and loosened with tools such as pneumatic picks before it can be unloaded.

[0003] The difficulty of unloading increases the labor intensity and operation risks. The catalyst in the hydrogenation unit is in a sulfided state after operation, and contains flammable substances such as hydrogen and oil gas. Careless unloading can easily lead to fire and other risks. To break the stuck catalyst, the operator needs to enter the narrow space in the reactor, and the labor intensity needs to be reduced as much as possible to protect the operator.

[0004] In order to reduce labor intensity and increase safety factor, vacuum suction and other methods have been used to unload the catalyst on the top of the reactor in recent years. However, when processing coking oil products, dense cake-like coke is often formed on the top of the bed, which cannot be unloaded by vacuum suction. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides a catalyst grading and filling method for hydrogenation of easily coking oil products, which uses an auxiliary catalyst with a larger porosity to separate the main catalyst, and utilizes a special grading and filling method to cleverly achieve the separation of the coked catalyst, reduce the labor required for unloading the catalyst, and reduce the maintenance cost of the hydrogenation device.

[0006] In order to achieve the above technical objectives, the technical solution of the present invention is as follows:

[0007] The present invention provides a catalyst grading and filling method for hydrogenation of easily coking oil products, which comprises the following steps: arranging a grading and filling section at the inlet section of a reactor, dividing the space of the grading and filling section into a plurality of main regions parallel to the material flow direction and auxiliary regions isolating the main regions, wherein the auxiliary regions extend axially along the material flow direction in the reactor but do not extend to the end of the reactor, the void ratio of the auxiliary regions is 0.40-0.80, preferably 0.45-0.70, and more preferably 0.45-0.60, and the void ratio of the main regions is smaller than that of the auxiliary regions.

[0008] The void ratio refers to the ratio of the void volume between catalyst particles to the total volume of the catalyst bed after the catalyst is loaded into the reactor. The determination method is well known to those skilled in the art.

[0009] It should be understood by those skilled in the art that the inlet section of the reactor is the end where the oil product enters the reactor. Specifically, the downstream reactor refers to the top of the reactor, the upstream reactor refers to the bottom of the reactor, the intermediate feed reactor and the gas-liquid countercurrent reactor refer to the inlet end in the flow direction of the oil product, and the same applies to other reactor types. The end of the reactor refers to the end along the material flow direction.

[0010] Further, the cross section of the auxiliary region is of any shape, which can be regular or irregular; the gradation method of the present invention is to facilitate the unloading of the agent after coking, and the characteristics of the liquid phase reaction process must also be considered. In order to avoid too much bias due to different catalyst porosity, the volume occupied by the auxiliary region is as small as possible, and its distribution mode is based on better isolation of the main region. Therefore, as one of the more preferred specific embodiments, the auxiliary region is arranged in a grid shape to isolate each main region, and the width of the grid is 20-500 mm, preferably 30-300 mm, and further preferably 40-150 mm; and the size of each main region is designed to be easy to unload from the reactor port when unloading, and when unloading, the catalyst with a larger porosity in the auxiliary region is first broken to obtain a dispersed main region catalyst coke block, so that it is easy to unload. Further, based on the total volume of the gradation loading section, the volume occupied by the auxiliary region accounts for 10-60%, preferably 10-45%, and more preferably 15-30%.

[0011] Furthermore, in the graded packing section, on any cross section of the reactor, the sum of the cross-sectional areas of the auxiliary regions is 2-70%, preferably 5-50%, and more preferably 15-30% of the cross-sectional area of ​​the reactor.

[0012] Further, as a preferred specific embodiment, the main regions are separated from each other, and the auxiliary regions are continuously filled in the remaining regions, similar to the shape of honeycomb briquettes. The main regions are inserted between the auxiliary regions as evenly as possible, and the cross-section of the main regions is any shape, specifically, a rectangle, a circle, a triangle, a parallelogram or its approximate shape, or other irregular shapes.

[0013] Further, the diameter or thickness of the main region is no more than 3000 mm, preferably no more than 800 mm, and more preferably no more than 500 mm. The thickness refers to the maximum distance in any direction relative to the main region with an irregular cross section.

[0014] Furthermore, in order to avoid logistics short-circuiting, the auxiliary region does not extend to the end of the reactor. Therefore, the catalyst bed height of the graded packing section accounts for 1%-95% of the entire reactor bed height, preferably 3%-60%, and more preferably 4%-50%.

[0015] Furthermore, the porosity of the main region is 0.10-0.50, preferably 0.20-0.40, and most preferably 0.20-0.35.

[0016] Further, one or more hydrogenation catalysts I are loaded in the auxiliary region, which are hollow particles and / or toothed particles. Hollow particles include but are not limited to five-hole spheres, six-hole spheres, seven-hole spheres, Raschig rings, cylindrical strips with three holes inside, cylindrical strips with five holes inside, round cakes with seven holes inside, round cakes with nine holes inside, etc.; toothed particles include but are not limited to three-tooth spheres, five-tooth spheres, six-tooth spheres, four-tooth strips, five-tooth strips, etc.; hollow toothed particles include but are not limited to one-hole three-tooth spheres, two-hole three-tooth spheres, three-hole three-tooth spheres, three-hole four-tooth spheres, one-hole five-tooth strips, three-hole five-tooth strips, seven-hole three-tooth strips, etc. More specifically, the particle size of the hydrogenation catalyst I is 2.0-55.0 mm, preferably 3.0-30.0 mm.

[0017] Furthermore, one or more hydrogenation catalysts II are loaded in the main region, and the hydrogenation catalysts II are porous particles; more specifically, the particle size of the hydrogenation catalysts II is 0.5-4.0 mm, preferably 0.8-3.0 mm.

[0018] Further, the rest of the reactor is filled with a conventional hydrogenation catalyst, the voidage of which is not greater than the voidage of the main region in the graded packing section. Preferably, the rest of the reactor is filled with the hydrogenation catalyst II loaded in the main catalyst.

[0019] Furthermore, the mass content of the hydrogenation active metal in the hydrogenation catalyst I, calculated as oxide, is 10%-90%, preferably 15%-60%, and more preferably 17%-40% of the hydrogenation catalyst II used in combination with the same grade.

[0020] Furthermore, the hydrogenation active metal in the hydrogenation catalyst I, hydrogenation catalyst II and the conventional hydrogenation catalyst loaded in the rest of the reactor involved in the above method is selected from at least one of Fe, Co, Ni, Cu, Zn, Cr, Mo and W, preferably at least one of Fe, Ni, Co, Mo and W, and more preferably Mo and Ni.

[0021] Furthermore, the hydrogenation catalyst I comprises a carrier material and a hydrogenation active metal, wherein the weight ratio of the hydrogenation active metal in terms of oxide is 5%-30% of the catalyst, and the carrier material is selected from at least one of activated carbon, alumina, silica, magnesium oxide, zirconium oxide, titanium oxide and molecular sieves, preferably at least one of alumina and silica.

[0022] Further, the hydrogenation catalyst I is prepared by a supported catalyst preparation method well known to those skilled in the art. More specifically, the carrier material is extruded, dried and calcined, and then impregnated with the hydrogenation active metal, and then dried and calcined. As a more specific embodiment, the extrusion molding is to blend the carrier material with a peptizing agent, an extrusion aid, etc., mix them evenly, and extrude them on an extruder or other molding machine to form hollow particles, including but not limited to five-hole spheres, six-hole spheres, seven-hole spheres, Raschig rings, cylindrical strips with three holes inside, cylindrical strips with five holes inside, round cakes with seven holes inside, and round cakes with nine holes inside, etc.; or to form particles with teeth, including but not limited to three-tooth spheres, five-tooth spheres, six-tooth spheres, four-tooth strips, five-tooth strips, etc.; or to form hollow particles with teeth, including but not limited to one-hole three-tooth spheres, two-hole three-tooth spheres, three-hole three-tooth spheres, three-hole four-tooth spheres, one-hole five-tooth strips, three-hole five-tooth strips, seven-hole three-tooth strips, etc. The impregnation is preferably an equal volume impregnation, in which the extruded carrier is impregnated with an equal volume of the stable salt solution of the hydrogenation active metal; the two dryings in the above preparation process are both dried at 70-150°C for 1-24 hours, and the two calcinations are both calcined at 300-600°C for 1-10 hours.

[0023] The hydrogenation catalyst II and the conventional hydrogenation catalyst are catalysts for oil hydrogenation that are well known to those skilled in the art and can achieve desulfurization, and are selected from at least one of a supported catalyst and an unsupported catalyst. The supported catalyst generally includes a carrier and a hydrogenation active component, and a catalyst modified on this basis, and the mass content of the hydrogenation active component in terms of metal oxide is 15%-40% based on the total weight of the catalyst, preferably 20%-35%. The unsupported catalyst includes at least the necessary binder and the hydrogenation active component, and the mass content of the hydrogenation active component in terms of metal oxide is 30%-80% based on the total weight of the catalyst, preferably 40%-65%.

[0024] Furthermore, the carrier in the supported catalyst and the binder in the unsupported catalyst are inorganic refractory oxides, specifically, at least one selected from oxides of elements of Group II, Group III, Group IV and Group IVB of the periodic table, more specifically, at least one selected from silica and alumina; further, the carrier or binder also includes a material formed after modifying the above-mentioned inorganic refractory oxide, and the purpose of the modification includes but is not limited to enhancing the strength of the catalyst, improving the activity of the catalyst, etc., such as modifying with modifying elements such as B, P, F, and the weight percentage of the modified elements is 0.8wt%-8wt% based on the weight of the modified carrier or binder.

[0025] Further, it is easy for a person skilled in the art to obtain the hydrogenation catalyst II and the conventional hydrogenation catalyst. As one of the specific embodiments, the supported catalyst is to extrude an inorganic refractory oxide, impregnate the hydrogenation active component after drying and calcining, and then dry and calcine to obtain the hydrogenation catalyst component with desulfurization activity. As a more specific embodiment, the extrusion molding is to blend the adsorbent porous material with a peptizing agent, an extrusion aid, etc., mix them evenly, and extrude them on an extruder. Preferably, it is a strip with a round, oval, three-leaf clover or four-leaf clover cross section, or a spherical particle obtained by rolling a ball, oil column molding, etc.; the impregnation is preferably an equal volume impregnation, and the stable salt solution of the hydrogenation active component is impregnated on the extruded carrier in an equal volume; the two dryings in the above preparation process are both dried at 70-150°C for 1-24 hours, and the two calcinations are both calcined at 300-600°C for 1-10 hours. The non-supported catalyst is a uniform catalyst prepared by the hydrogenation active component and the binder component by including but not limited to co-precipitation.

[0026] It should be understood by those skilled in the art that the grading filling method of the present invention is applicable to the treatment of any oil raw material, and is particularly applicable to oil containing substances that are easy to coke, and the raw materials include but are not limited to ethylene cracking gasoline, coking naphtha, catalytic gasoline, Fischer-Tropsch synthetic oil, coking diesel, catalytic diesel, high-dry point straight-run diesel, wax oil, residual oil, coal tar, coal hydrogenation generated oil, etc. In the hydrofining process, substances that are easy to coke in oil products, such as olefins and aromatics, are easily dehydrogenated and condensed when heated, and the catalyst particles are adhered together, making it difficult to unload. For example, hydrogenation of coking gasoline causes coking at the material inlet of the hydrofining reactor, and it is very difficult to unload the catalyst at the end of the operation. The large pancake-shaped coked catalyst at the material inlet needs to be broken and loosened with tools such as pneumatic picks before it can be unloaded.

[0027] Traditional technology uses a single catalyst, and the coking material generated easily sticks the catalyst particles together to form a cake with high strength. In the technical solution of the present invention, a graded filling section is set at the entrance of the reactor, and a catalyst with a lower porosity is filled in the main area. The contact between the catalyst particles is closer, and the strength of the block formed by coking is higher. An auxiliary area is set between the main areas, and a catalyst with a higher porosity is filled therein. The contact area between the catalyst particles is smaller, and the strength of the block formed by coking is lower. When the coked catalyst needs to be unloaded, use a tool such as a jackhammer to first break the auxiliary area with lower strength, separate the main area, and unload the catalyst in an easier way.

[0028] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 . A schematic cross-sectional view of the reactor after the catalyst D1 and catalyst A1 are graded and loaded in Example 7;

[0030] Figure 2 . A schematic cross-sectional view of the reactor after the catalyst D2 and the catalyst A2 are graded and loaded in Example 8;

[0031] Figure 3 . Schematic diagram of the cross section of the reactor after the catalyst D3 and catalyst A3 are graded and loaded in Example 9. DETAILED DESCRIPTION

[0032] The following non-limiting embodiments may enable a person skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way.

[0033] In Examples 1-3, hydrogenation catalysts II D1-D3 with smaller porosity were prepared:

[0034] Example 1

[0035] Preparation of hydrogenation catalyst D1:

[0036] Take 1000 grams of macroporous aluminum hydroxide, add nitric acid and water to obtain a paste mixture with an HNO3 content of 2.2% and a water content of 65%. Extrude the above mixture on an extruder to obtain clover-shaped strips with a diameter of 1.5 mm, dry at 100°C for 2 hours, and then calcine at 600°C for 5 hours to obtain a carrier. Take ammonium heptamolybdate and nickel nitrate to prepare an aqueous solution, and impregnate an equal volume of the above carrier for 30 minutes to obtain wet strips with a molybdenum oxide content of 24% and a nickel oxide content of 4% (calculated on a dry basis after calcination). Dry at 100°C for 2 hours, and then calcine at 550°C for 2 hours to obtain catalyst D1, which has a high desulfurization activity.

[0037] The bed voidage of catalyst D1 was measured to be 0.24.

[0038] Example 2

[0039] Preparation of hydrogenation catalyst D2:

[0040] Take 1000 grams of macroporous amorphous silica-alumina, add nitric acid and water to obtain a paste mixture with an HNO3 content of 2.3% and a water content of 68%, extrude the above mixture on an extruder to obtain cylindrical strips with a diameter of 1.5 mm, dry at 80°C for 18 hours, and then calcine at 500°C for 9 hours to obtain a carrier, prepare an aqueous solution of ammonium heptamolybdate and nickel nitrate, and impregnate an equal volume of the above carrier for 30 minutes to obtain wet strips with a molybdenum oxide content of 27% and a nickel oxide content of 5% (based on the dry basis after calcination), dry at 100°C for 2 hours, and then calcine at 500°C for 9 hours to obtain catalyst D2 with high desulfurization activity.

[0041] It was determined that the bed voidage of catalyst D2 was 0.34.

[0042] Example 3

[0043] Preparation of hydrogenation catalyst D3:

[0044] Take 1000 grams of aluminum hydroxide containing 0.9% fluorine, add nitric acid and water to obtain a paste mixture with an HNO3 content of 1.3% and a water content of 60%, extrude the above mixture on an extruder to obtain four-leaf clover columnar strips with a diameter of 1.5 mm, dry at 140°C for 6 hours, and then roast at 550°C for 2 hours to obtain a carrier, take ammonium heptamolybdate and cobalt nitrate to prepare an aqueous solution, and impregnate an equal volume of the above carrier for 30 minutes to obtain wet strips with a molybdenum oxide content of 16% and a cobalt oxide content of 3% (calculated on a dry basis after roasting), dry at 100°C for 2 hours, and then roast at 580°C for 3 hours to obtain catalyst D3 with high desulfurization activity.

[0045] It was determined that the bed voidage of catalyst D3 was 0.21.

[0046] In Examples 4-6, hydrogenation catalysts IA1-A3 with larger porosity were prepared:

[0047] Example 4

[0048] Preparation of hydrogenation catalyst A1:

[0049] 1000 g of small pore aluminum hydroxide was added with nitric acid and water to obtain a paste mixture with a HNO3 content of 2% and a water content of 70%. The mixture was extruded on an extruder to obtain a hollow cylindrical bar with a diameter of 6 mm and a hollow part diameter of 3 mm. The carrier was obtained by drying at 100°C for 2 hours and then calcining at 550°C for 5 hours. Nickel nitrate was prepared into an aqueous solution and impregnated with an equal volume of the above carrier for 30 minutes to obtain a wet bar with a nickel oxide content of 3% (calculated on a dry basis after calcination). The wet bar was dried at 100°C for 2 hours and then calcined at 550°C for 2 hours to obtain catalyst A1.

[0050] It was determined that the bed porosity of catalyst A1 was 0.56 and the total metal oxide content was 10.7% of that of the corresponding catalyst D1.

[0051] Example 5

[0052] Preparation of hydrogenation catalyst A2:

[0053] 1000 g of small-pore amorphous silica-alumina was added with nitric acid and water to obtain a mixture with a HNO3 content of 1.1% and a water content of 13%. The mixture was pressed on a tablet press to obtain five-hole round cake-shaped particles with a diameter of 12 mm and a height of 6 mm, and an inner hole diameter of 1.5 mm. The particles were dried at 70°C for 20 hours and then calcined at 580°C for 9 hours to obtain a carrier. Ferric nitrate and ammonium heptamolybdate were prepared into an aqueous solution, and an equal volume of the above carrier was impregnated for 30 minutes to obtain a wet strip with a molybdenum oxide content of 12% and an iron oxide content of 4% (calculated on a dry basis after calcination). The wet strip was dried at 100°C for 2 hours and then calcined at 580°C for 8 hours to obtain catalyst A2.

[0054] It was determined that the bed porosity of catalyst A2 was 0.46 and the total metal oxide content was 50% of that of the corresponding catalyst D2.

[0055] Example 6

[0056] Preparation of hydrogenation catalyst A3:

[0057] Take 1000g of small-pore aluminum hydroxide containing 3% silicon oxide, add nitric acid and water to obtain a paste mixture with a HNO3 content of 2.8% and a water content of 80%, extrude the above mixture on an extruder to obtain a honeycomb strip with a diameter of 20mm, with 23 square grids evenly distributed inside, dry at 130℃ for 6 hours, and then calcine at 490℃ for 7 hours to obtain a carrier. Take zinc nitrate to prepare an aqueous solution, impregnate an equal volume of the above carrier for 30 minutes, obtain a wet strip with a zinc oxide content of 3% (calculated on a dry basis after calcination), dry at 100℃ for 2 hours, and then calcine at 490℃ for 6 hours to obtain catalyst A3.

[0058] It was determined that the bed porosity of catalyst A3 was 0.59, and the total metal oxide content was 15.7% of that of the corresponding catalyst D3.

[0059] Example 7

[0060] Catalyst D1 and Catalyst A1 were loaded into a cylindrical hydrogenation reactor:

[0061] The reactor is a co-current reactor. The oil products to be hydrogenated and hydrogen enter from the upper part of the reactor, and the post-reaction logistics flow out from the lower part. When filling, the catalyst D1 with a smaller porosity is first evenly filled in the lower part of the reactor. The catalyst bed occupies 70% of the reactor height; then the catalyst D1 and catalyst A1 are continuously filled in the upper graded filling section according to the scheme of the present invention. For the graded filling part, from the cross-sectional view, the reactor is divided into a number of square spaces by intersecting horizontal and vertical lines, and the separated areas are partially filled with catalyst D1 as the main area, and the remaining continuous parts are filled with catalyst A1 as the auxiliary area, such as Figure 1 Except for the edge part, the side length of the middle square grid main area is 400mm, and the catalyst A1 grid width is 40mm.

[0062] Example 8

[0063] Catalyst D2 and Catalyst A2 were loaded into a cylindrical hydrogenation reactor:

[0064] The reactor is an upflow reactor. The oil product to be hydrogenated and hydrogen enter from the lower part of the reactor, and the reacted logistics flows out from the upper part. When filling, first fill the catalyst D2 and catalyst A2 in the lower part of the reactor according to the gradation of the present invention. From the cross-section, the reactor is divided into several parallelogram spaces by the crossed horizontal and vertical lines. The catalyst D2 is filled in the parallelogram space as the main area, and the catalyst A2 is filled on the dividing line as the auxiliary area. Figure 2 As shown. The maximum thickness of the parallelogram is 600 mm, and the width of the dividing line is 100 mm. The height of the catalyst bed in the graded loading section is 40% of the total height of the reactor bed. Then, the catalyst D2 is evenly loaded on the graded catalyst bed.

[0065] Example 9

[0066] Catalyst D3 and catalyst A3 were loaded into a cylindrical hydrogenation reactor:

[0067] The reactor is an upflow reactor. The oil product to be hydrogenated and hydrogen enter from the bottom of the reactor, and the post-reaction logistics flows out from the top. When filling, first fill the catalyst D3 and catalyst A3 in the lower part of the reactor according to the gradation of the present invention. From the cross-section, the reactor is divided into multiple sectors by three straight lines passing through the center of the circle. The catalyst D3 is filled in the sector space as the main area, and the catalyst A3 is filled on the dividing line as the auxiliary area. Figure 3 As shown. The sector radius is 2000mm, and the dividing line width is 150mm. The rest is filled with catalyst D3, and the catalyst bed height of the graded filling section is 60% of the total height of the reactor bed. Then, catalyst D3 is evenly filled on the graded catalyst bed.

[0068] The reactor filled with the graded configurations of Examples 7, 8 and 9 was used for the hydrogenation reaction of easily coking oil products. The sulfur content in the oil products after the hydrogenation reaction did not show a significant change, indicating that the bias flow generated in the reactor after the above-mentioned graded configurations did not affect the product quality and met the production requirements. After the device had been running for a certain period of time, the oil product inlet part was severely coked and needed to be unloaded. At this time, a pneumatic pick or other tool was used to first break the auxiliary area with lower strength, separate the main area, and unload the catalyst in an easier way.

[0069] Compared with the conventional loading method in the prior art, i.e., loading the entire reactor with catalyst D1, or catalyst D2, or catalyst D3, the sulfur content of the generated oil in the technical solution of the present invention is slightly reduced, but still meets the production requirements. However, it is obvious that the loading method of the present invention is easier to unload the catalyst and is more suitable for the hydrogenation reaction of easily coking oil products.

Claims

1. A catalyst grading and loading method for hydrogenation of easily coking oil products, It is characterized in that A graded packing section is arranged at the inlet section of the reactor, and the space of the graded packing section is divided into a plurality of main areas parallel to the material flow direction and auxiliary areas separating the main areas, wherein the auxiliary areas extend axially along the material flow direction in the reactor but do not extend to the end of the reactor, and the auxiliary areas use an auxiliary catalyst with a larger porosity to separate the main catalyst in the main area, the porosity of the auxiliary areas is 0.40-0.80, and the porosity of the main area is smaller than that of the auxiliary areas; the auxiliary areas are arranged in a grid shape to isolate the main areas, the main areas are separated from each other, and the auxiliary areas form continuous packing in the remaining areas; the catalyst bed height of the graded packing section accounts for 1%-95% of the total reactor bed height; and conventional hydrogenation catalyst is filled in the remaining part of the reactor, and its porosity is not greater than that of the main area in the graded packing section.

2. The catalyst grading and loading method according to claim 1, It is characterized in that The void ratio of the auxiliary region is 0.45-0.

70.

3. The catalyst grading and loading method according to claim 2, It is characterized in that The void ratio of the auxiliary region is 0.45-0.

60.

4. The catalyst grading and loading method according to claim 1, It is characterized in that The auxiliary area is arranged in a grid shape with a grid width of 20-500 mm.

5. The catalyst grading and loading method according to claim 4, It is characterized in that The width of the grid is 30-300 mm.

6. The catalyst grading and loading method according to claim 5, It is characterized in that The width of the grid is 40-150 mm.

7. The catalyst grading and loading method according to claim 1, It is characterized in that Based on the total volume of the graded filling section, the volume occupied by the auxiliary area accounts for 10-60%.

8. The catalyst grading and loading method according to claim 7, It is characterized in that Based on the total volume of the graded packing section, the volume occupied by the auxiliary area accounts for 10-45%.

9. The catalyst grading and loading method according to claim 8, It is characterized in that Based on the total volume of the graded filling section, the volume occupied by the auxiliary area accounts for 15-30%.

10. The catalyst grading and loading method according to claim 7, It is characterized in that In the graded packing section, on any cross section of the reactor, the sum of the cross-sectional areas of the auxiliary regions is 2-70% of the cross-sectional area of ​​the reactor.

11. The catalyst grading and loading method according to claim 10, It is characterized in that In the graded packing section, on any cross section of the reactor, the sum of the cross-sectional areas of the auxiliary regions is 5-50% of the cross-sectional area of ​​the reactor.

12. The catalyst grading and loading method according to claim 11, It is characterized in that In the graded packing section, on any cross section of the reactor, the sum of the cross-sectional areas of the auxiliary regions is 15-30% of the cross-sectional area of ​​the reactor.

13. The catalyst grading and loading method according to claim 4, It is characterized in that The cross section of the main area may be rectangular, circular, triangular, parallelogram, or other irregular shapes.

14. The catalyst grading and loading method according to claim 13, It is characterized in that The diameter or thickness of the main area does not exceed 3000 mm.

15. The catalyst grading and loading method according to claim 14, It is characterized in that The diameter or thickness of the main area does not exceed 800 mm.

16. The catalyst grading and loading method according to claim 15, It is characterized in that The diameter or thickness of the main area does not exceed 500 mm.

17. The catalyst grading and loading method according to claim 1, It is characterized in that The catalyst bed height of the graded filling section accounts for 3%-60% of the entire reactor bed height.

18. The catalyst grading and loading method according to claim 17, It is characterized in that The catalyst bed height of the graded filling section accounts for 4%-50% of the entire reactor bed height.

19. The catalyst grading and loading method according to claim 1, It is characterized in that The void fraction of the main region is 0.10-0.

50.

20. The catalyst grading and loading method according to claim 19, It is characterized in that The void fraction of the main region is 0.20-0.

40.

21. The catalyst grading and loading method according to claim 20, It is characterized in that The void fraction of the main region is 0.20-0.

35.

22. The catalyst grading and loading method according to claim 1, It is characterized in that The auxiliary region is filled with one or more hydrogenation catalysts I, which are hollow particles and / or particles with teeth.

23. The catalyst grading and loading method according to claim 22, It is characterized in that The particle size of the hydrogenation catalyst I is 2.0-55.0 mm.

24. The catalyst grading and loading method according to claim 22, It is characterized in that One or more hydrogenation catalysts II are loaded in the main region, and the particle size of the hydrogenation catalyst II is 0.5-4.0 mm.

25. The catalyst grading and loading method according to claim 24, It is characterized in that The mass content of the hydrogenation active metal in the hydrogenation catalyst I, calculated as oxide, is 10% to 90% of that in the hydrogenation catalyst II used in combination with the same grade.

26. The catalyst grading and loading method according to claim 24, It is characterized in that The hydrogenation active metal in the hydrogenation catalyst I, hydrogenation catalyst II and the conventional hydrogenation catalyst loaded in the rest of the reactor is selected from at least one of Fe, Co, Ni, Cu, Zn, Cr, Mo and W.

27. The catalyst grading and loading method according to claim 26, It is characterized in that The hydrogenation catalyst I comprises a carrier material and a hydrogenation active metal, wherein the weight ratio of the hydrogenation active metal in terms of oxide is 5%-30% of the catalyst, and the carrier material is selected from at least one of activated carbon, aluminum oxide, silicon oxide, magnesium oxide, zirconium oxide, titanium oxide and molecular sieve.

28. The catalyst grading and loading method according to claim 26, It is characterized in that The hydrogenation catalyst II and the conventional hydrogenation catalyst are catalysts used in oil hydrogenation and capable of achieving desulfurization, and are selected from at least one of a supported catalyst and a non-supported catalyst.

29. The catalyst grading and loading method according to claim 1, It is characterized in that The oil products that are easy to form tar are ethylene cracking gasoline, coker naphtha, catalytic gasoline, Fischer-Tropsch synthetic oil, coker diesel, catalytic diesel, wax oil, residual oil, coal tar or coal hydrogenation oil.