A high-hardness and high-density W-Ti alloy and preparation method thereof

Through the oscillating hot pressing sintering and oscillating hot forging processes, the problems of long sintering temperature and long time in the preparation of W-Ti alloys are solved, and W-Ti alloys with high density and hardness are achieved, reducing energy consumption and costs, and significantly improving material properties.

CN116574949BInactive Publication Date: 2024-10-08UNIV OF SHANGHAI FOR SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310452926.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure CN116574949B_ABST
    Figure CN116574949B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of metal material preparation, and specifically relates to a high-hardness and high-density W-Ti alloy and a preparation method thereof. The preparation method of the high-hardness and high-density W-Ti alloy of the present invention comprises the steps of cold pressing, oscillating hot pressing sintering, and oscillating hot forging of the W-Ti composite powder in sequence. The present invention matches the oscillating hot pressing sintering with the oscillating hot forging treatment under a specific process, and the obtained W-Ti alloy has few internal defects, fine and uniform grains, and high density. Performance test experiments show that the density of the W-Ti alloy of the present invention is greater than 99%, and the Vickers hardness can reach up to 800HV, which is significantly better than the existing W-Ti alloy materials, has excellent comprehensive performance, and can better meet the preparation and application requirements of high-performance W-Ti alloys.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal material preparation, and specifically relates to a high-hardness and high-density W-Ti alloy and a preparation method thereof. Background Art

[0002] With the rapid development of micro-mechanical manufacturing, tungsten-titanium alloys are widely used in device coating in the fields of semiconductors, photovoltaic solar energy, etc. due to their high density, moderate film stress, excellent surface flatness and thermochemical stability.

[0003] When W-Ti alloy is used as a diffusion barrier at the junction of semiconductor metals, due to the large difference in density and melting point between the components of W-Ti alloy, the conventional powder metallurgy method (i.e., ordinary hot pressing and sintering) is prone to component segregation and uneven composition, thereby affecting the performance of the alloy. Therefore, the main preparation methods of existing tungsten-titanium alloys include vacuum hot pressing (HP), hot isostatic pressing (HIP), and thermal explosion consolidation combustion synthesis (CSA-HEC). Existing researchers have studied and compared these methods. Among them, the number of contaminated particles introduced into the vacuum hot pressing method is the least, and the hot isostatic pressing method is the most. However, the hot pressing sintering temperature is high, the grains are easy to grow, and the energy consumption is high. For hot isostatic pressing, its production cost is high and the production efficiency is low. However, due to its inherent defects, hot explosion forming is prone to sample cracking, especially there are certain dangers in the operation process, which limits its application.

[0004] The latest report shows that using controllable dynamic pressure instead of traditional static force during sintering and processing can effectively improve the uniformity of the organization, increase more driving force, and improve the density of the product. However, although oscillating hot pressing sintering can achieve higher density, it still requires higher sintering temperature, pressure or longer sintering time, which can easily lead to slow densification and abnormal grain growth, thereby significantly reducing the performance of the alloy. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a high-hardness and high-density W-Ti alloy, so as to solve the problems of high sintering temperature and pressure or long sintering time, slow densification, abnormal grain growth and low alloy hardness in the existing W-Ti alloy preparation.

[0006] Another object of the present invention is to provide a high-hardness and high-density W-Ti alloy, which has both high density and high hardness and is suitable for the application of W-Ti alloy in high-performance semiconductor metal joints.

[0007] To achieve the above object, the preparation method of the high hardness and high density W-Ti alloy of the present invention adopts the technical scheme as follows:

[0008] A method for preparing a high-hardness and high-density W-Ti alloy comprises the following steps:

[0009] (1) cold pressing the W-Ti composite powder to obtain a cold pressed green body;

[0010] (2) placing the cold-pressed green body in an oscillating hot-pressing sintering furnace for temperature-raising and constant-pressure treatment, and maintaining the temperature after the temperature reaches the set temperature T1, performing oscillating hot-pressing sintering during the temperature-keeping period, and then cooling to obtain a W-Ti preform;

[0011] (3) placing the W-Ti preform in an oscillating hot pressing sintering furnace for temperature-raising and constant pressure treatment, and maintaining the temperature after the temperature reaches the set temperature T2, performing oscillating hot forging treatment during the temperature maintenance period, and then cooling to obtain a high-hardness and high-density W-Ti alloy;

[0012] Wherein, in step (2), the process conditions of oscillating hot pressing sintering are: setting temperature T1 to 600-800°C, median pressure to 10-30 MPa, amplitude to 1-10 MPa, frequency to 1-10 Hz, and holding time to 0.5-1.0 h;

[0013] In step (3), the process conditions of the oscillation hot forging treatment are: setting the temperature T2 to 900-1100°C, the median pressure to 40-60MPa, the amplitude to 5-20MPa, the frequency to 5-20Hz, and the holding time to 0.5-1.0h.

[0014] The method for preparing a high-hardness and high-density W-Ti alloy of the present invention adopts an oscillating hot pressing sintering + oscillating hot forging process to prepare the W-Ti refractory alloy. The present invention first prepares a W-Ti preform body by oscillating hot pressing sintering, and then performs an oscillating hot forging treatment on the preform body to obtain a high-hardness and high-density W-Ti alloy.

[0015] Among them, hot pressing is the process of preparing a block of pre-sintered powder under the action of temperature and pressure. The hot pressing process adopted by the present invention is oscillating hot pressing sintering, that is, the powder is sintered and prepared under a thermal field and a cyclic force field, so as to obtain a sintered green body with high density and refined grains faster and better. However, the green body sintered by oscillating hot pressing has certain organizational defects and low density. The present invention further promotes green body processing deformation to a great extent, eliminates internal organizational defects, and inhibits grain growth while improving density, thereby improving material properties.

[0016] Hot forging is the process of processing and deforming bulk materials under temperature and pressure. The hot forging process in the present invention is oscillating hot forging, which is different from the conventional constant pressure hot forging method (usually the heat field is open, the temperature field cannot be kept at a constant temperature, the forging pressure field is a constant pressure, and it is not easy to deform the blank). The present invention is the first to put the bulk blank obtained by oscillating hot pressing sintering into an oscillating hot pressing sintering furnace (constant temperature and dynamically controllable pressure) for oscillating hot forging treatment. By maintaining a constant temperature and controllable oscillation frequency, it can effectively promote large-scale processing deformation of the blank (volume shrinkage, relative density increase) and microstructure refinement (particle size growth is inhibited), thereby obtaining a high-hardness, high-density W-Ti alloy.

[0017] Furthermore, the present invention adopts a combination of oscillating hot pressing sintering and oscillating hot forging processes, which can obtain W-Ti alloys with fine grains, high density, and especially high hardness in a very short time, at a relatively low temperature and pressure. Compared with the prior art, it can effectively reduce energy consumption, save process time, and reduce process costs, with obvious advantages.

[0018] In step (1), preferably, the mass percentage composition of the W-Ti composite powder is: 90% W, 10% Ti. The W-Ti alloy prepared from the W-Ti composite powder having such a composition is suitable for use as a diffusion barrier layer at semiconductor metal connections.

[0019] Further preferably, the W-Ti composite powder is prepared by mixing W powder and Ti powder by mechanical ball milling; the purity of the W powder is ≥99.5%, and the purity of the Ti powder is ≥99.9%; the average particle size of the W-Ti composite powder is 1 to 3 μm. The mixing of the powders and the control of the particle size are achieved by ball milling, thereby facilitating the subsequent sintering preparation of the alloy. More preferably, the average particle size of the W-Ti composite powder is 2 μm.

[0020] In step (1), preferably, the cold pressing pressure is 5-8 MPa and the time is 5-10 min. Cold pressing can be performed by conventional methods in the art, such as loading the W-Ti composite powder into a pre-set sintered graphite mold to perform cold pressing of the powder.

[0021] In step (2), the temperature-raising and constant-pressure treatment is to raise the temperature under a constant pressure to reach the set temperature T1; the constant pressure adopted in the temperature-raising and constant-pressure treatment in step (2) is 4 to 6 MPa, and the heating rate is 6 to 10°C / min.

[0022] In order to avoid the influence of low density or large particle size on the subsequent hot forging effect, as a preferred solution, in step (2), the density of the W-Ti preform is 60% to 85%. By controlling the density of the W-Ti preform, the subsequent oscillating hot forging process can obtain a blank with a more suitable processing deformation space, thereby better taking into account the comprehensive improvement effect of the oscillating hot pressing sintering + oscillating hot forging process on the density and hardness of the alloy.

[0023] Furthermore, in step (3), the temperature-raising and constant-pressure treatment is to raise the temperature under a constant pressure to reach a set temperature T2; the constant pressure adopted in the temperature-raising and constant-pressure treatment in step (3) is 4 to 6 MPa, and the heating rate is 6 to 10°C / min.

[0024] In order to reduce oxidation of the alloy material and ensure the performance improvement effect, preferably, the oscillation hot pressing sintering in step (2) and the oscillation hot forging treatment in step (3) are both carried out under vacuum conditions.

[0025] Furthermore, in step (2) and step (3), the cooling is furnace cooling.

[0026] The high-hardness and high-density W-Ti alloy of the present invention is prepared by the preparation method as described above.

[0027] The W-Ti alloy obtained by the present invention through oscillating hot pressing sintering and oscillating hot forging treatment has few internal defects, fine and uniform grains, and high density. Performance tests show that the W-Ti alloy obtained by the oscillating hot pressing sintering + oscillating hot forging combined with the present invention has a density greater than 99%, a Vickers hardness of up to 800HV, excellent comprehensive performance, significantly better than the existing W-Ti alloy materials, and can better meet the application requirements of high-performance W-Ti alloys. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The actual picture of the deformation of the W-Ti alloy samples prepared before and after the oscillation hot forging treatment in Examples 1 to 3 of the present invention;

[0029] Figure 2 The microstructure morphology of the W-Ti alloy samples prepared before and after the oscillation hot forging treatment in Examples 1 to 3 of the present invention is shown;

[0030] Figure 3 The density result diagram of the W-Ti alloy samples prepared before and after forging in Examples 1 to 3 of the present invention;

[0031] Figure 4 The hardness result diagram of the W-Ti alloy samples prepared before and after forging in Examples 1 to 3 of the present invention;

[0032] Figure 5 The density result diagram of the W-Ti alloy samples prepared in Example 3 of the present invention and Comparative Examples 1 to 2;

[0033] Figure 6 This is a graph showing the hardness results of the W-Ti alloy samples prepared in Example 3 of the present invention and Comparative Examples 1 to 2. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is further described below in conjunction with specific embodiments and drawings, but the protection scope of the present invention is not limited thereto.

[0035] The preparation method of the high-hardness and high-density W-Ti alloy of the present invention comprises the following steps:

[0036] (1) cold pressing the W-Ti composite powder to obtain a cold pressed green body;

[0037] (2) placing the cold-pressed green body in an oscillating hot-pressing sintering furnace for temperature-raising and constant-pressure treatment, and maintaining the temperature after the temperature reaches the set temperature T1, performing oscillating hot-pressing sintering during the temperature-keeping period, and then cooling to obtain a W-Ti preform;

[0038] (3) placing the W-Ti preform in an oscillating hot pressing sintering furnace for temperature-raising and constant pressure treatment, and maintaining the temperature after the temperature reaches the set temperature T2, performing oscillating hot forging treatment during the temperature maintenance period, and then cooling to obtain a high-hardness and high-density W-Ti alloy;

[0039] Wherein, in step (2), the process conditions of oscillating hot pressing sintering are: setting temperature T1 to 600-800°C, median pressure to 10-30 MPa, amplitude to 1-10 MPa, frequency to 1-10 Hz, and holding time to 0.5-1.0 h;

[0040] In step (3), the process conditions of the oscillation hot forging treatment are: setting the temperature T2 to 900-1100°C, the median pressure to 40-60MPa, the amplitude to 5-20MPa, the frequency to 5-20Hz, and the holding time to 0.5-1.0h.

[0041] Further preferably, the W-Ti composite powder is prepared by mixing W powder and Ti powder by mechanical ball milling; the purity of the W powder is ≥99.5%, and the purity of the Ti powder is ≥99.9%; and the average particle size of the W-Ti composite powder is 1 to 3 μm.

[0042] In step (1), preferably, the cold pressing pressure is 5 to 8 MPa and the time is 5 to 10 min.

[0043] In step (2), the temperature-raising and constant-pressure treatment is to raise the temperature under a constant pressure to reach the set temperature T1; the constant pressure adopted in the temperature-raising and constant-pressure treatment in step (2) is 4 to 6 MPa, and the heating rate is 6 to 10°C / min.

[0044] As a preferred solution, in step (2), the density of the W-Ti preform is 60% to 85%. The shape and size of the sintered preform can be adjusted according to actual needs, which can achieve the equivalent technical effects of the present invention. In the following embodiments, the W-Ti preform is a cylinder with a diameter of 20 to 60 mm and a thickness of 3 to 15 mm.

[0045] Furthermore, in step (3), the temperature-raising and constant-pressure treatment is to raise the temperature under a constant pressure to reach a set temperature T2; the constant pressure adopted in the temperature-raising and constant-pressure treatment in step (3) is 4 to 6 MPa, and the heating rate is 6 to 10°C / min.

[0046] In the following embodiments, for the purpose of illustration and to facilitate the performance test of subsequent samples, in step (3), before the temperature-controlled pressure treatment, the W-Ti preform is also cut. Specifically, the W-Ti preform is cut into small cylinders smaller than the W-Ti preform, and the diameter of the small cylinder is 10 to 20 mm. In other embodiments, the W-Ti preform can be directly subjected to the temperature-controlled pressure treatment and the oscillating hot forging treatment without cutting, which can achieve the technical effects equivalent to those of the present invention.

[0047] In order to reduce the oxidation of the alloy material and ensure the performance improvement effect, the oscillation hot pressing sintering in step (2) and the oscillation hot forging treatment in step (3) are both carried out under vacuum conditions. In step (2) and step (3), the cooling is furnace cooling.

[0048] Example 1

[0049] The high hardness and high density W-Ti alloy of this embodiment is prepared by the following steps:

[0050] (1) placing W-Ti composite powder into a pre-sintered graphite mold (φ40 mm) for cold pressing to obtain a cold pressed green body;

[0051] Among them, the W-Ti composite powder is 90W-10Ti (mass fraction) powder, and the W-Ti composite powder is made by mixing W powder and Ti powder through high-energy ball milling; the purity of W powder is ≥99.5%, and the purity of Ti powder is ≥99.9%; the average particle size of the W-Ti composite powder is 2μm; the pressure of cold pressing is 5MPa, and the time is 5min.

[0052] (2) The cold-pressed green body is placed in an oscillating hot pressing sintering furnace, and the furnace chamber is closed and vacuumized. The green body is then subjected to a temperature-controlled constant pressure treatment (the constant pressure is 5 MPa, and the heating rate is 8°C / min). After the temperature reaches the set temperature T1, it is kept warm. During the warm-keeping period, oscillating hot pressing sintering is performed (during the oscillating hot pressing sintering process, the set temperature T1 is 800°C, the median pressure is 30 MPa, the amplitude is 5 MPa, the frequency is 10 Hz, and the warm-keeping time is 0.5 h). After the warm-keeping is completed, the green body is cooled to room temperature with the furnace, and is taken out from the sintering furnace to obtain a W-Ti preform. The obtained W-Ti preform has a density of 72%, is cylindrical in shape, has a diameter of 40 mm, and a thickness of 8 mm.

[0053] (3) Cut the W-Ti preform into small cylinders with a diameter of 15±0.05 mm, then put the cut samples into a graphite mold with a diameter of 30 mm (without carbon paper), and load the furnace; close the furnace door and evacuate, then perform temperature and constant pressure treatment (constant pressure is 5 MPa, and the heating rate is 8°C / min), and keep the temperature after reaching the set temperature T2. During the insulation period, perform oscillation hot forging treatment (during the oscillation hot forging process, the set temperature T2 is 900°C, the median pressure is 40 MPa, the amplitude is 5 MPa, the frequency is 10 Hz, and the insulation time is 0.5 h). After the insulation is completed, the blank is cooled to room temperature with the furnace to obtain the high hardness and high density W-Ti alloy of Example 1.

[0054] Example 2

[0055] The high hardness and high density W-Ti alloy of this embodiment is prepared by the following steps:

[0056] (1) placing W-Ti composite powder into a pre-sintered graphite mold (φ40 mm) for cold pressing to obtain a cold pressed green body;

[0057] Among them, the W-Ti composite powder is 90W-10Ti (mass fraction) powder, and the W-Ti composite powder is made by mixing W powder and Ti powder through high-energy ball milling; the purity of W powder is ≥99.5%, and the purity of Ti powder is ≥99.9%; the average particle size of the W-Ti composite powder is 2μm; the pressure of cold pressing is 5MPa, and the time is 5min.

[0058] (2) The cold-pressed green body is placed in an oscillating hot pressing sintering furnace, and the furnace chamber is closed and vacuumized. The green body is then subjected to a temperature-controlled constant pressure treatment (the constant pressure is 5 MPa, and the heating rate is 8°C / min). After the temperature reaches the set temperature T1, it is kept warm. During the warm-keeping period, oscillating hot pressing sintering is performed (during the oscillating hot pressing sintering process, the set temperature T1 is 800°C, the median pressure is 30 MPa, the amplitude is 5 MPa, the frequency is 10 Hz, and the warm-keeping time is 0.5 h). After the warm-keeping is completed, the green body is cooled to room temperature with the furnace, and is taken out from the sintering furnace to obtain a W-Ti preform. The obtained W-Ti preform has a density of 72%, is cylindrical in shape, has a diameter of 40 mm, and a thickness of 8 mm.

[0059] (3) Cut the W-Ti preform into small cylinders with a diameter of 15±0.05 mm, then put the cut samples into a graphite mold with a diameter of 30 mm (without carbon paper), and load the furnace; close the furnace door to evacuate, then perform temperature and constant pressure treatment (constant pressure is 5 MPa, and the heating rate is 8°C / min), and keep the temperature after reaching the set temperature T2. During the insulation period, perform oscillation hot forging treatment (during the oscillation hot forging process, the set temperature T2 is 1000°C, the median pressure is 40 MPa, the amplitude is 5 MPa, the frequency is 10 Hz, and the insulation time is 0.5 h). After the insulation is completed, the blank is cooled to room temperature with the furnace to obtain the high hardness and high density W-Ti alloy of Example 2.

[0060] Example 3

[0061] The high hardness and high density W-Ti alloy of this embodiment is prepared by the following steps:

[0062] (1) placing W-Ti composite powder into a pre-sintered graphite mold (φ40 mm) for cold pressing to obtain a cold pressed green body;

[0063] Among them, the W-Ti composite powder is 90W-10Ti (mass fraction) powder, and the W-Ti composite powder is made by mixing W powder and Ti powder through high-energy ball milling; the purity of W powder is ≥99.5%, and the purity of Ti powder is ≥99.9%; the average particle size of the W-Ti composite powder is 2μm; the pressure of cold pressing is 5MPa, and the time is 5min.

[0064] (2) The cold-pressed green body is placed in an oscillating hot pressing sintering furnace, and the furnace chamber is closed and vacuumized. The green body is then subjected to a temperature-controlled constant pressure treatment (the constant pressure is 5 MPa, and the heating rate is 8°C / min). After the temperature reaches the set temperature T1, it is kept warm. During the warm-keeping period, oscillating hot pressing sintering is performed (during the oscillating hot pressing sintering process, the set temperature T1 is 800°C, the median pressure is 30 MPa, the amplitude is 5 MPa, the frequency is 10 Hz, and the warm-keeping time is 0.5 h). After the warm-keeping is completed, the green body is cooled to room temperature with the furnace, and is taken out from the sintering furnace to obtain a W-Ti preform. The obtained W-Ti preform has a density of 72%, is cylindrical in shape, has a diameter of 40 mm, and a thickness of 8 mm.

[0065] (3) Cut the W-Ti preform into small cylinders with a diameter of 15±0.05 mm, then put the cut samples into a graphite mold with a diameter of 30 mm (without carbon paper), and load the furnace; close the furnace door to evacuate, then perform temperature and constant pressure treatment (constant pressure is 5 MPa, and the heating rate is 8°C / min), and keep the temperature after reaching the set temperature T2. During the insulation period, perform oscillation hot forging treatment (during the oscillation hot forging process, the set temperature T2 is 1100°C, the median pressure is 40 MPa, the amplitude is 5 MPa, the frequency is 10 Hz, and the insulation time is 0.5 h). After the insulation is completed, the blank is cooled to room temperature with the furnace to obtain the high hardness and high density W-Ti alloy of Example 3.

[0066] Comparative Example 1

[0067] The W-Ti alloy of comparative example 1 is prepared by ordinary hot pressing sintering (powder metallurgy) + oscillation hot forging process. The specific preparation process is basically the same as that of Example 3, and the difference between the two is that: in step (2), ordinary hot pressing sintering is used instead of oscillation hot pressing sintering, and the temperature of ordinary hot pressing sintering is 1100°C, the pressure is 30MPa, and the sintering time is 0.5h. Among them, during ordinary hot pressing sintering, the sintering temperatures used in the present invention are 900, 1000, and 1100°C. After testing, it was found that the W-Ti alloy material sintered at 1100°C has the best performance, so 1100°C is used as the sintering temperature of comparative example 1.

[0068] Comparative Example 2

[0069] The W-Ti alloy of comparative example 2 is prepared by oscillating hot pressing sintering + conventional hot forging process. The specific preparation process is basically the same as that of Example 3, and the only difference between the two is that in step (2), the parameters of oscillating hot pressing sintering are: temperature 1100°C, median pressure 60MPa, amplitude 20MPa, frequency 20Hz, and time 0.5h. In step (3), a conventional hot forging process is used instead of the oscillating hot forging process, and the conditions of the conventional hot forging process are: temperature 1100°C, pressure 60MPa, and time 0.5h. Among them, the oscillating hot pressing sintering and conventional hot forging process conditions of comparative example 2 are the process conditions with the best performance of W-Ti alloy preferably obtained within a certain parameter range of the present invention.

[0070] Test Example 1 Deformation and Microstructure Analysis

[0071] The deformation of the samples obtained in Examples 1 to 3 of the present invention before and after the oscillation hot forging treatment was compared. The deformation comparison results are shown in the figure below. Figure 1 The microstructure morphology of the W-Ti samples obtained before and after oscillation hot forging in Examples 1 to 3 was further compared. The results are shown in Figure 2 shown.

[0072] in, Figure 1 From left to right in the figure are the actual pictures before forging, after forging at 900°C of Example 1, after forging at 1000°C of Example 2, and after forging at 1100°C of Example 3. Figure 2 In the figure, the microstructure of the sample before hot forging is shown in Figure a, the microstructure of the sample after hot forging of Example 1 is shown in Figure b, the microstructure of the sample after hot forging of Example 2 is shown in Figure c, and the microstructure of the sample after hot forging of Example 3 is shown in Figure d.

[0073] Depend on Figure 1 From the physical comparison diagram of W-Ti specimens before and after forging, it can be seen that with the increase of hot forging temperature, the deformation also increases.

[0074] Further through Figure 2 From the comparison of the microstructures of the samples of Examples 1 to 3 before and after forging, it can be seen that the porosity of the samples before forging is relatively high, while the porosity is significantly reduced after forging, which greatly removes the pores, eliminates the internal defects of the organization, and improves the density of the material. Among them, the improvement of the sample of Example 3 is the most obvious.

[0075] Test Example 2 Comparative Analysis of the Properties of the Alloys of Examples 1 to 3

[0076] The density of the W-Ti alloy samples before forging and after forging in Examples 1 to 3 was analyzed by the Archimedes density displacement method. The results are as follows: Figure 3 The Vickers hardness of the W-Ti alloy samples before forging and after forging in Examples 1 to 3 was further analyzed using a HV-30 Vickers hardness tester. The results are shown in Figure 4 shown.

[0077] like Figure 3 As shown in the figure, with the increase of sintering temperature, the density also increases. When the sintering temperature is 1100℃, the density reaches the highest, reaching about 99%, almost reaching full density. Compared with the density before forging, the improvement effect is quite obvious.

[0078] Depend on Figure 4 It can be seen that the hardness of the sample before forging is only about 260HV, and after oscillation hot forging, the hardness of the sample has been greatly improved, especially at 1100℃, the hardness has exceeded 800HV, which is equivalent to three times the hardness of the sample before forging, and the hardness improvement effect is significant. At the same time, compared with Examples 1 to 3, as the sintering temperature increases, the hardness also increases, and when the sintering temperature is 1100℃, the hardness is the highest.

[0079] The above results also confirm that the green body sintered by oscillating hot pressing has certain structural defects, low density and poor performance. The present invention further introduces oscillating hot forging, which can eliminate internal structural defects to a large extent, inhibit grain growth while improving density, and greatly improve the hardness performance of the material.

[0080] Experimental Example 3 Comparative Analysis of Alloy Properties of Example 3 and Comparative Examples 1-2

[0081] In this test example, the density and hardness of the W-Ti alloys prepared in Example 3 and Comparative Examples 1 to 2 were analyzed using the Archimedes density displacement method and the HV-30 Vickers hardness tester. The results are as follows: Figure 5 , 6 shown.

[0082] Depend on Figure 5 The density analysis results show that the density of the W-Ti alloy obtained in Example 3 of the present invention is as high as 99.1%, which is better than the density of the alloys in Comparative Examples 1 and 2 (98.6% and 98.2%, respectively).

[0083] In particular, by Figure 6 It can be seen that the hardness of the W-Ti alloy obtained in Example 3 of the present invention is as high as 800 HV 30 , an increase of 57% compared to comparative example 1, and an increase of 70% compared to comparative example 2.

[0084] In summary, the present invention adopts a combination of oscillating hot pressing sintering + oscillating hot forging process to obtain a W-Ti alloy with fine grains and high density, and greatly improves the hardness performance of the W-Ti alloy. At the same time, compared with other processes, the temperature and pressure of the present invention are lower, which is conducive to reducing energy consumption. It has obvious advantages and is very suitable for the preparation and application of high-performance W-Ti alloys.

Claims

1. A method for preparing a high-hardness and high-density W-Ti alloy, characterized in that: The steps include: (1) cold pressing a W-Ti composite powder to obtain a cold pressed green body; the W-Ti composite powder has a mass percentage composition of: 90% W and 10% Ti; (2) placing the cold-pressed green body in an oscillating hot-pressing sintering furnace for temperature-raising and constant-pressure treatment, and maintaining the temperature after the temperature reaches the set temperature T1. During the temperature-keeping period, oscillating hot-pressing sintering is performed, and then cooling is performed to obtain a W-Ti preform; (3) placing the W-Ti preform in an oscillating hot pressing sintering furnace for temperature-raising and constant pressure treatment, and maintaining the temperature after the temperature reaches the set temperature T2. During the temperature maintenance period, an oscillating hot forging treatment is performed, and then cooling is performed to obtain a high-hardness and high-density W-Ti alloy; Wherein, in step (2), the process conditions of oscillating hot pressing sintering are: setting temperature T1 to 800°C, median pressure to 30MPa, amplitude to 5MPa, frequency to 10Hz, and holding time to 0.5h; In step (3), the process conditions of the oscillation hot forging treatment are: setting the temperature T2 to 1100°C, the median pressure to 40 MPa, the amplitude to 5 MPa, the frequency to 10 Hz, and the holding time to 0.5 h.

2. The method for preparing a high-hardness and high-density W-Ti alloy according to claim 1, characterized in that: In step (1), the W-Ti composite powder is prepared by mixing W powder and Ti powder through mechanical ball milling; the purity of the W powder is ≥99.5%, and the purity of the Ti powder is ≥99.9%; and the average particle size of the W-Ti composite powder is 1-3 μm.

3. The method for preparing a high-hardness and high-density W-Ti alloy according to claim 1, characterized in that: In step (1), the cold pressing pressure is 5-8 MPa and the time is 5-10 min.

4. The method for preparing a high-hardness and high-density W-Ti alloy according to claim 1, characterized in that: In step (2), the temperature-raising and constant-pressure treatment is to raise the temperature under a constant pressure to reach the set temperature T1; the constant pressure adopted in the temperature-raising and constant-pressure treatment in step (2) is 4-6 MPa, and the heating rate is 6-10°C / min.

5. The method for preparing a high-hardness and high-density W-Ti alloy according to claim 1, characterized in that: In step (2), the density of the W-Ti preform is 60% to 85%.

6. The method for preparing a high-hardness and high-density W-Ti alloy according to claim 1, characterized in that: In step (3), the temperature-raising and constant-pressure treatment is to raise the temperature under a constant pressure to reach the set temperature T2; the constant pressure adopted in the temperature-raising and constant-pressure treatment in step (3) is 4-6 MPa, and the heating rate is 6-10°C / min.

7. The method for preparing a high-hardness and high-density W-Ti alloy according to any one of claims 1 to 6, characterized in that: The oscillation hot pressing sintering in step (2) and the oscillation hot forging treatment in step (3) are both carried out under vacuum conditions.

8. The method for preparing a high-hardness and high-density W-Ti alloy according to any one of claims 1 to 6, characterized in that: In step (2) and step (3), the cooling is furnace cooling.

9. A high-hardness and high-density W-Ti alloy prepared by the preparation method according to any one of claims 1 to 8.