Thick film slurry suitable for filter immersion silver spinning process and preparation method thereof and filter
By optimizing the formula and process of silver conductor paste, combining low glass content and high temperature wetting agents, the wetting, uniformity and adhesion of the silver layer in the silver-splitting process is solved, and efficient silver layer preparation is achieved and bubbles are reduced. Problems of risk and insufficient adhesion.
Patent Information
- Application Number
- CN202211730851.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-12-30
AI Technical Summary
In the existing silver-spray process, silver paste is difficult to balance various properties, resulting in poor wetting of small deep holes, uneven edge thickness when high-speed silver-spraying, secondary flow after drying, easy silver layer to fall off and bubble risk, and so on. High glass content leads to insufficient adhesion and conductivity.
The silver conductor paste consists of spherical silver powder, sheet silver powder, microcrystalline silver powder, low glass powder, high temperature wetting agent, organic carrier and hydrogenated rosin ester solution. By optimizing the formulation and process flow, it combines low glass content and high temperature wetting. Wetting agent to achieve uniformity and adhesion of the silver layer.
It improves the wetting property of the silver layer, the uniformity of edge and surface thickness, reduces the risk of secondary flow and shedding after drying, ensures the conductivity and adhesion of the silver layer, and reduces the possibility of bubbles appearing.
Smart Images

Figure CN116580871B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electronic materials, and in particular to a thick film slurry suitable for a filter silver immersion-spinning process and a preparation method thereof. Background Art
[0002] Ceramic dielectric filters are small in size and have a simple molding process. They have been popular in 5G communications in recent years. The preparation process of 5G ceramic dielectric filters mainly includes batching, granulation, dry pressing, sintering, metallization, etc. Among them, metallization is one of the key technologies of ceramic dielectric filters and has a direct impact on the performance and reliability of the filter. The metallization process currently commonly used in industry is the silver burning process, that is, a layer of silver paste is coated on the surface of the ceramic filter, and then dried and sintered at high temperature. In this way, the surface of the ceramic filter is covered with a layer of silver film. There are four main ways to apply silver paste in the silver burning process: silver spraying, silver immersion, screen printing, and silver injection.
[0003] Among them, the existing silver immersion and spinning process is mainly as follows: first, the ceramic device is placed in a special fixture (silver spinning machine component), then immersed in silver slurry and retained for a certain period of time, then the fixture is taken out of the silver slurry, and silver is spun at high speed, and the sample is taken out of the fixture using a robotic arm for subsequent drying and sintering. Summary of the invention
[0004] The invention provides a thick film slurry (or silver conductor slurry) suitable for a filter immersion and spinning silver process. The slurry can balance various properties and has good process matching.
[0005] The technical solution of the present invention is as follows:
[0006] A silver conductor slurry, suitable for filter leaching and spinning silver process, mainly composed of the following raw materials in percentage by weight:
[0007] Spherical silver powder 20% to 70%, flake silver powder 10% to 40%, microcrystalline silver powder 10% to 30%;
[0008] Glass powder: 0.1%~0.5%;
[0009] High temperature wetting agent: 1-3%;
[0010] Organic carrier: 1% to 10%;
[0011] Hydrogenated rosin ester solution: 0.5-3%;
[0012] Organic diluent 3%~15%.
[0013] The "mainly composed of the following raw materials in weight percentage" mentioned in the present invention means that the silver conductor paste can achieve the technical effects of the present invention as long as it includes the components and contents listed above. However, in addition to the components listed above, the silver conductor paste of the present invention may also contain a small amount of other components that do not affect the realization of the technical effects of the present invention after being added, such as but not limited to silicon dioxide, copper oxide, etc.
[0014] In a preferred embodiment of the silver conductor paste, the average particle size of the spherical silver powder is 0.5 to 2.5 μm, and the tap density is 3.0 to 7.0 g / cm 3 The average particle size of the flaky silver powder is 0.5-5.0 μm, and the tap density is 3.0-7.0 g / cm 3 The average particle size of the microcrystalline silver powder is 0.2 to 2 μm, and the tap density is 1 to 3 g / cm 3 .
[0015] In a preferred embodiment of the silver conductor paste, the main body of the high temperature wetting agent is crystalline bismuth oxide with a particle size of 0.2 to 3 μm. That is to say, the high temperature wetting agent can be only bismuth oxide, or the high temperature wetting agent has a relatively large content of bismuth oxide, and can also contain a small amount of other oxides, such as at least one selected from silver oxide, copper oxide and other oxides, and the content of other oxides is preferably selected so as not to affect the effect of the high temperature wetting agent. The role of the high temperature wetting agent is to cooperate with the low content of glass powder, so that the silver paste still meets the adhesion requirements when the glass powder content is reduced.
[0016] In a preferred embodiment of the silver conductor paste, the glass powder is selected from glass powder with a low expansion coefficient. For example, the glass powder is Bi-Zn-B-Si glass, and the particle size of the glass powder is 0.2-2 μm. The selected glass powder has an expansion buffering effect on crystalline bismuth oxide. However, the present invention can also use other types of glass powder.
[0017] In a preferred embodiment of the silver conductor paste, the organic vehicle is composed of the following raw materials in weight percentage: 5% to 25% resin and 75% to 95% organic solvent, wherein the resin is any one or two of polyester resin, polyvinyl butyral, and ethyl cellulose. The resin in the organic vehicle does not select or include hydrogenated rosin ester.
[0018] In a preferred embodiment of the silver conductor paste, the hydrogenated rosin ester solution comprises one or more hydrogenated rosin esters with a softening point of 80 to 120° C., and the content of the hydrogenated rosin ester solution is 0.5 to 2 wt %. Further preferably, the hydrogenated rosin ester solution comprises one or more rosin esters with a softening point of 110 to 115° C., and further, the weight percentage of the hydrogenated rosin ester solution is not greater than 1.5%.
[0019] Furthermore, the hydrogenated rosin ester solution is composed of the following raw materials in weight percentage: 30-60% hydrogenated rosin ester and 40-70% organic solvent.
[0020] It is preferred that the organic carrier and the hydrogenated rosin ester solution use the same organic solvent to reduce influencing factors. Alternatively, the organic carrier and the hydrogenated rosin ester solution may use different solvents.
[0021] In a preferred embodiment of the silver conductor paste, the organic solvent is any one of terpineol, diethylene glycol dibutyl ether, butyl carbitol acetate, or a mixture of two or more thereof.
[0022] In a preferred embodiment of the silver conductor paste, the organic diluent is a low boiling point solvent, such as diethylene glycol dimethyl ether, dibasic acid ester (DBE), dimethylformamide, etc., which is used for dilution and viscosity adjustment. The boiling point temperature of the low boiling point solvent described in the present invention is set according to the drying process requirements, and the boiling point can usually be selected to be lower than 230°C.
[0023] In the present invention, the organic carrier and the hydrogenated rosin ester solution can be prepared separately, or prepared by adding resin and hydrogenated rosin ester into the same solvent system according to the above-mentioned proportion.
[0024] Based on the same inventive concept, the present invention also provides a method for preparing the above-mentioned silver conductor slurry. The prepared silver conductor slurry is suitable for the filter leaching and spinning silver process. The preparation method comprises the following steps:
[0025] (I) Preparation of glass powder, organic carrier and hydrogenated rosin ester solution
[0026] Preparation of glass powder: weigh the oxides in proportion to the composition of the glass powder, mix them thoroughly, and evenly melt them at 1000-1200°C, quench the evenly melted glass to obtain coarse glass particles, and centrifugally ball-mill the coarse glass particles to obtain powder with an average particle size of 0.2-2 μm, and then dry them to obtain glass powder;
[0027] Preparation of organic carrier: Heat the organic solvent to 60-90°C, add the resin under stirring, continue stirring until dissolved, and finally form a transparent homogeneous solution to obtain the organic carrier;
[0028] Preparation of hydrogenated rosin ester solution: heat the organic solvent to 60-90°C, add hydrogenated rosin ester under stirring, continue stirring until dissolved, and finally form a transparent homogeneous solution to obtain hydrogenated rosin ester solution;
[0029] (ii) Preparation of silver conductor paste: the organic carrier prepared above, the hydrogenated rosin ester solution prepared above, the spherical silver powder, the flaky silver powder, the microcrystalline silver powder, the glass powder prepared above, the high-temperature wetting agent, and part of the organic diluent are mixed according to the formula ratio of the aforementioned silver conductor paste product, and after being mixed evenly, they are fully ground and rolled. The remaining organic diluent is added to the semi-finished product after rolling, and the viscosity is adjusted to a suitable value, filtered, and then packaged to obtain the silver conductor paste; or, the organic carrier prepared above, the hydrogenated rosin ester solution prepared above, the spherical silver powder, the flaky silver powder, the microcrystalline silver powder, the glass powder prepared above, and the high-temperature wetting agent are mixed according to the formula ratio of the aforementioned silver conductor paste product, and after being mixed evenly, they are fully ground and rolled. The organic diluent is added to the semi-finished product after rolling to adjust the viscosity to a suitable value, filtered, and then packaged to obtain the silver conductor paste.
[0030] For the preparation of glass powder, generally speaking, the melting time of the glass powder can be selected as 1 hour.
[0031] For the preparation of glass powder, generally speaking, a two-roll mill is used for quenching.
[0032] For the preparation of glass powder, generally speaking, centrifugal ball milling can be carried out in a corundum tank, and the processing time can be 4 to 8 hours.
[0033] For the preparation of glass powder, generally speaking, the drying temperature can be selected to be 100°C.
[0034] For the preparation of the organic carrier or hydrogenated rosin ester solution, generally speaking, the time for continuous stirring until dissolution can be selected to be 2 to 4 hours.
[0035] In the above step (i), the preparation of the glass powder, the preparation of the organic carrier and the preparation of the hydrogenated rosin ester solution are not prioritized.
[0036] For the preparation of the silver conductor paste, a stirring disperser may generally be used for the mixing process.
[0037] For the preparation of silver conductor paste, grinding rolling is usually carried out on a three-roll mill.
[0038] For the preparation of silver conductor paste, the amount of organic diluent added in the first addition is usually set and selected according to the processing requirements of grinding roller equipment such as three-roll mill, and the amount added in the second addition is set and selected according to the respective silver leaching and spinning process requirements of different manufacturers.
[0039] For the preparation of the silver conductor slurry, the filtration is preferably performed with a filter cloth with a mesh size of 400 or more to obtain a silver conductor slurry with a fineness of ≤10 μm. The smaller the fineness, the smoother and finer the silver layer.
[0040] In the method for preparing the silver conductor paste of the present invention, the preparation of the organic vehicle and the preparation of the hydrogenated rosin ester solution can also be replaced by adding the resin and the hydrogenated rosin ester into the same solvent system for preparation.
[0041] Based on the same inventive concept, the present invention also provides a filter using the above silver conductor paste.
[0042] In the silver conductor paste of the present invention, the hydrogenated rosin ester solution is added as a special additive, thereby optimizing the silver immersion and silver throwing process of the silver conductor paste. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 This is a structure of an exemplary dielectric filter described in an embodiment of the present invention. DETAILED DESCRIPTION
[0044] The silver paste formula used in the current silver immersion and silver throwing process (or silver immersion and silver throwing process) is: flake silver powder + microcrystalline silver powder + spherical silver powder + glass powder + ethyl cellulose resin (EC resin). The silver paste product is difficult to balance various properties and has poor process matching. Among them, in the selection of silver paste thixotropic properties, the current mainstream method is to choose high thixotropic, but high thixotropic silver paste has the following advantages and disadvantages:
[0045] First, at the end of silver throwing and during the drying process, the storage modulus is large and the shaping is good;
[0046] Second, in the silver immersion process, the fluidity is poor (interfacial tension is large), and the wetting of small deep holes (D = 0.5mm; depth ~ 4mm) is poor. Since the dielectric filter product has a large number of small deep holes (see Figure 1 ), poor wetting of small deep holes leads to poor product quality;
[0047] Third, during the silver throwing process, due to the high thixotropy, the silver edge thickness is low and the silver surface thickness is uneven when the silver is thrown at a high speed (when the silver throwing speed is fast, the shear of the slurry is large, the slurry with high thixotropy has lower viscosity and low slurry hanging rate).
[0048] If you choose low thixotropic silver paste, it will cause the following problems:
[0049] First, at the end of silver throwing and during the drying process, the loss modulus is large, the fluidity is good, it is easy to flow again, the edge thickness is low, and the silver surface thickness is uneven;
[0050] Second, it cannot meet the requirements of the silver impregnation and spinning process; the softening point of ethyl cellulose resin is high, and the silver layer of the dried filter sample is easily damaged during the subsequent process stages and the transportation process of packaging and shipment.
[0051] In addition, the current silver paste has the following defects in performance characteristics:
[0052] (1) Most existing products use a high glass content formula (1-3%) to meet the adhesion requirements, but too much glass content will deteriorate the insertion loss value.
[0053] (2) When the sintered silver layer of the existing product is too thick, the resin at the bottom of the silver layer is not completely decomposed and is not discharged in time, so it decomposes and expands below the surface of the metallized silver layer, resulting in the risk of bubbles in the silver layer. When there are bubbles in the silver layer, the performance deteriorates. Therefore, it is difficult for existing products to achieve a thicker silver layer.
[0054] Therefore, there is an urgent need for a silver paste solution that can solve the following problems or achieve the following goals:
[0055] 1. When immersion silver is realized, the silver paste has good wettability for small deep holes.
[0056] 2. When realizing high-speed silver throwing, ensure the thickness of the edge silver layer and the uniformity of the silver layer thickness.
[0057] 3. Solve the problem of secondary flow of slurry on the product and uneven thickness (silver accumulation in severe cases) at the end of high-speed silver throwing and drying.
[0058] 4. Solve the problem that the silver layer is easy to fall off after collision during the transportation of dried products.
[0059] 5. To achieve a thicker silver layer without bubbles or other poor appearance.
[0060] 6. While achieving a low glass content formula design, it also meets the adhesion requirements and reduces the adverse effects on the insertion loss value.
[0061] The present invention provides a thick film slurry (or silver conductor slurry) suitable for filter immersion silver spinning process and its preparation method, which can solve the above problems. The silver conductor slurry is mainly composed of the following raw materials in weight percentage:
[0062] Spherical silver powder 20% to 70%, flake silver powder 10% to 40%, microcrystalline silver powder 10% to 30%;
[0063] Glass powder: 0.1%~0.5%;
[0064] High temperature wetting agent: 1-3%;
[0065] Organic carrier: 1% to 10%;
[0066] Hydrogenated rosin ester solution: 0.5-3%;
[0067] Organic diluent 3%~15%.
[0068] The high temperature wetting agent is preferably crystalline bismuth oxide, and the organic diluent is selected as butyl carbitol in the following examples.
[0069] The silver conductor paste provided by the present invention comprises an organic carrier and a hydrogenated rosin ester solution, which is a dual-carrier system. The present invention simultaneously achieves the following through the technical solution of the dual-carrier system:
[0070] 1. Add hydrogenated rosin ester solution to slow down the fluidity, select spherical silver powder + short chain (low softening point) resin to achieve low thixotropy, thereby reducing the interfacial tension and improving the wetting effect of the slurry on the small pores of the 5G ceramic body.
[0071] 2. The addition of hydrogenated rosin ester solution increases the resin content in the slurry, thereby increasing the viscosity of the slurry during high-speed silver throwing, ensuring the thickness of the edge silver layer and the uniformity of the silver layer thickness, and a high slurry hanging rate.
[0072] 3. Take advantage of the low viscosity of the hydrogenated rosin ester solution after adding it into the silver conductor slurry to slow down the fluidity of the slurry. After the high-speed silver throwing is completed and during drying, the secondary flow of the slurry on the product is slowed down to prevent uneven thickness (silver piling in severe cases).
[0073] 4. Select hydrogenated rosin ester with a lower softening point in the hydrogenated rosin ester solution. The viscosity of hydrogenated rosin ester with a low softening point dissolved in the solvent is lower. Therefore, under the same carrier viscosity, the amount of hydrogenated rosin ester with a low softening point that can be added is higher, thereby increasing the total resin content. The resin can fix the silver powder and prevent the silver layer from falling off after collision during the drying and transportation process.
[0074] 5. Taking advantage of the good high-temperature decomposition property of the hydrogenated rosin ester in the hydrogenated rosin ester solution, it is not easy to generate bubbles when the sintered silver layer is thick (there are no bubbles in the silver layer of 30um after sintering).
[0075] Furthermore, the silver conductor paste of the present invention also uses low glass content + high temperature wetting agent, which can meet the customer's requirements for adhesion. At the same time, low glass content (low impurities) and high temperature wetting agent (promoting silver particle metallization) will increase the conductivity of the silver layer, reduce the loss value, and reduce the adverse effects on the loss value.
[0076] In this article, the range expressed by "a value to another value" is a summary expression method to avoid listing all the values in the range one by one in the specification. Therefore, the description of a specific numerical range covers any value in the numerical range and a smaller numerical range defined by any value in the numerical range, just as if the arbitrary value and the smaller numerical range were explicitly written in the specification.
[0077] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of protection of the present invention. Improvements and adjustments made by those skilled in the art in practical applications according to the present invention still belong to the scope of protection of the present invention.
[0078] Example 1
[0079] According to the formula 1-10 in Table 1, the silver conductor paste was prepared using the following method:
[0080] 1. Preparation of glass powder: Weigh the oxides in proportion to the composition of the glass powder, mix them thoroughly, and then melt them at 1000-1200℃ for 1 hour. Use a two-roller mill to quench the evenly melted glass to obtain coarse glass particles, add them into a corundum tank and centrifuge them for 4-8 hours to obtain powder with an average particle size of 0.2-2μm, and then dry them at 100℃ to obtain glass powder. The formula of glass powder is as follows: Bi2O3: 63.6%; ZnO: 9.7%; B2O3: 9.0%; SiO2: 8.0%; CaO: 4.2%; Al2O3: 3.0%; BaO: 2.5%.
[0081] 2. Preparation of organic carrier: Heat the organic solvent (butyl carbitol) to 60-90°C, add ethyl cellulose resin in the ratio of ethyl cellulose (STD-10) to butyl carbitol = 15:85, and continue stirring for 2-4 hours until dissolved, and finally form a transparent homogeneous solution, which is the organic carrier. The preparation of the organic carrier in the comparative example refers to the above steps.
[0082] 3. Preparation of hydrogenated rosin ester solution: Heat the organic solvent butyl carbitol to 60-90°C, add hydrogenated rosin ester in sequence according to the ratio of hydrogenated rosin ester to butyl carbitol = 1:1 under stirring, and continue stirring for 2-4 hours until dissolved, and finally form a transparent homogeneous solution, which is the hydrogenated rosin ester solution. The preparation of the rosin solution in formula 10 refers to the above steps.
[0083] 4. Preparation method of silver paste: organic carrier, hydrogenated rosin ester solution, spherical silver powder, flaky silver powder, microcrystalline silver powder, glass powder, high temperature wetting agent, part of organic diluent are mixed with a stirring disperser according to the formula ratio of silver conductor paste, and after mixing evenly, they are fully ground and rolled on a three-roller mill, and the semi-finished product after rolling is added with the remaining organic diluent (10% butyl carbitol) to adjust to a suitable viscosity value, and filtered with a filter cloth of 400 mesh or more, and then packaged to obtain a silver conductor paste with a fineness of ≤10μm. Among them, the high temperature wetting agent used is crystalline bismuth oxide.
[0084] In the above silver leaching and spinning process, the ceramic body used is No. 21 ceramic (product number) and the Ca / Mg / Ti substrate is used.
[0085] The performance test method is as follows:
[0086] (1) Drying adhesion: drying temperature 150℃, time 10-15 minutes, 100 cuts with knife, 3M600 tape pulled vertically.
[0087] 4B: No silver layer falling off;
[0088] 5B: No silver layer is seen to fall off, and no obvious silver layer fall off is seen on the surface.
[0089] (2) Bubbles: The sample to be tested was sintered according to the standard sintering curve at 850°C for 10 minutes. The thickness of the silver layer was measured using an X-ray thickness gauge. The number of bubbles in the silver layer was observed using a microscope.
[0090] (3) Surface thickness / Sigma, edge thickness / Sigma: The filter sample is sliced, and the thickness of the filter surface and edges is tested using a 3D microscope, and its Sigma value is calculated.
[0091] (4) Adhesion: On the sintered silver surface, first stick a solder mask ring with an inner radius of 1 mm (with a circular hole in the middle), use 1 mm nickel-plated copper wire and SAC305 tin wire, apply flux to the area to be welded inside the solder mask ring, use a welding gun to melt the tin wire, and weld the nickel-plated copper wire to the welding area at 400°C within 1-2 seconds. Remove the welding gun, place the sample to be tested at room temperature, and use a tensile gauge to test the adhesion between the tin-plated copper wire and the silver layer.
[0092] The loss value test is completed at the product terminal.
[0093] The test results of formulas 1-10 are also shown in Table 1. Among them,
[0094] Formula 1 and Formula 6 were comparative examples without adding hydrogenated rosin ester solution;
[0095] Formula 2-5 and Formula 7-8 are embodiments, wherein the softening points of hydrogenated rosin ester in Formula 2-5 are different, Formula 7 provides different glass powder and butyl carbitol contents relative to Formula 4, and Formula 8 provides different butyl carbitol and hydrogenated rosin ester solution contents relative to Formula 4;
[0096] Formula 9 is a comparative example in which bismuth oxide is not added but silver oxide is added;
[0097] Formulation 10 is a comparative example in which rosin is added but no hydrogenated rosin ester is added.
[0098] The numbers after the hydrogenated rosin esters represent their respective softening points.
[0099] Table 1
[0100]
[0101]
[0102] Analysis of the test results in Table 1 shows that:
[0103] 1. The quality of drying adhesion is represented by 4B and 5B, where 4B and 5B represent the results of drying adhesion, and the larger the value, the better the drying adhesion performance. As can be seen from Table 1, the drying adhesion of Formula 1 and Formula 6 is slightly poor, and neither of these two formulas adds hydrogenated rosin ester solution. It can be seen that the present invention adds hydrogenated rosin ester solution to the silver conductor slurry, which optimizes the drying adhesion performance of the slurry.
[0104] 2. In terms of bubble performance, Formula 2 and Formula 10 show microbubbles, while Formula 3 and Formula 8 show slight bubbles. In Formula 2 and Formula 3, the softening point of hydrogenated rosin ester is relatively low. It can be seen that, under the same hydrogenated rosin ester content, as the softening point of rosin ester increases, its bubble performance becomes better. The hydrogenated rosin ester content in Formula 8 is higher than that in Formula 7 and Formula 4. It can be seen that hydrogenated rosin ester above a certain content will lead to a weakening of its bubble improvement effect. Formula 4 and Formula 10 respectively use different types of rosin, wherein Formula 4 uses hydrogenated rosin ester-110, and Formula 10 uses rosin. Their bubble performance is also different. Formula 4 shows no bubbles, while Formula 10 shows microbubbles. This shows that although they are of similar types, rosin cannot achieve the effect of hydrogenated rosin ester selected by the present invention.
[0105] 3. The four sets of values of filter surface thickness, surface thickness sigma, filter edge thickness, and edge thickness sigma can be compared.
[0106] The surface thickness of formulas 2-5, 7-8 as examples is significantly higher than that of formulas 1 and 6 as comparative examples. Formula 9 as a comparative example still using hydrogenated rosin ester but using silver oxide instead of bismuth oxide has a surface thickness higher than that of formulas 1 and 6 as comparative examples. The surface thickness of formula 10 using rosin instead of hydrogenated rosin ester is similar to that of formulas 1 and 6 as comparative examples.
[0107] The surface thickness sigma of formulas 2-5 and 7-8 is significantly smaller than that of formula 1 and formula 6. Formula 9 is a comparative example that still uses hydrogenated rosin ester but uses silver oxide instead of bismuth oxide. The surface thickness sigma is smaller than that of formula 1 and formula 6. The surface thickness sigma of formula 10 that uses rosin instead of hydrogenated rosin ester is similar to that of formula 1 and formula 6.
[0108] The filter edge thickness of formulas 2-5, 7-8 is significantly higher than that of formula 1 and formula 6. Formula 9 is a comparative example that still uses hydrogenated rosin ester but uses silver oxide instead of bismuth oxide. The filter edge thickness is higher than that of formula 1 and formula 6. The filter edge thickness of formula 10 that uses rosin instead of hydrogenated rosin ester is similar to that of formula 1 and formula 6.
[0109] The edge thickness sigma of formulas 2-5 and 7-8 is significantly smaller than that of formula 1 and formula 6. Formula 9, as a comparative example that still uses hydrogenated rosin ester but uses silver oxide instead of bismuth oxide, has an edge thickness sigma smaller than that of formula 1 and formula 6. The edge thickness sigma of formula 10 that uses rosin instead of hydrogenated rosin ester is similar to that of formula 1 and formula 6.
[0110] In summary, it can be seen that the average thickness of the embodiment formulations 2-5 and 7-8 is higher than that of the comparative example formulations 1 and 6, and the Sigma value is smaller, so the thickness performance of formulations 2 to 5 and 7-8 is better than that of formulations 1, 6 and 10.
[0111] 4. Adhesion data: It can be seen that the adhesion data of formulas 2-5, 7-8, and 10 are similar to that of formula 1, while the adhesion data of formulas 6 and 9 are poor. The improvement in adhesion is caused by low glass powder + bismuth oxide, while formula 6 does not add bismuth oxide, and formula 9 uses silver oxide instead of bismuth oxide, neither of which can improve the adhesion.
[0112] 5. From the loss value data, it can be seen that the loss values of Formula 1, Formula 6, and Formula 9 are higher than those of other formulas. The improvement in the loss value is caused by low glass powder + bismuth oxide, while Formula 1, Formula 6, and Formula 9 do not have this technical feature and therefore do not achieve the result of improved loss value.
[0113] Under the guidance of the present invention and the above-mentioned embodiments, it is easy for those skilled in the art to foresee that each raw material or its equivalent substitute, each processing method or its equivalent substitute listed or exemplified in the present invention can realize the present invention, and the upper and lower limit values and interval values of the parameters of each raw material and processing method can realize the present invention, and the embodiments are not listed one by one here.
Claims
1. A silver conductor slurry suitable for filter leaching and spinning silver process, characterized in that: It is mainly composed of the following raw materials in weight percentage: Spherical silver powder 20%~70%, flake silver powder 10%~40%, microcrystalline silver powder 10%~30%; Glass powder: 0.1%~0.5%; High temperature wetting agent: 1~3%; Organic carrier: 1% to 10%; Hydrogenated rosin ester solution: 0.5~2%; Organic diluent 3% to 15%; Wherein, the glass powder is a glass powder with a low expansion coefficient, the glass powder is a Bi-Zn-B-Si glass, and the particle size of the glass powder is 0.2 to 2 μm; The main body of the high temperature wetting agent is crystalline bismuth oxide with a particle size of 0.2-3 μm; The organic carrier is composed of the following raw materials in weight percentage: 5% to 25% resin and 75% to 95% organic solvent, wherein the resin is any one or two of polyester resin, polyvinyl butyral and ethyl cellulose; In the hydrogenated rosin ester solution, one or more rosin esters having a softening point of 110-115°C are selected; The hydrogenated rosin ester solution is composed of the following raw materials in weight percentage: 30-60% hydrogenated rosin ester and 40-70% organic solvent.
2. The silver conductive paste according to claim 1, characterized in that The spherical silver powder has an average particle size of 0.5 to 2.5 μm and a tap density of 3.0 to 7g / cm3 The average particle size of the flaky silver powder is 0.5 to 5.0 μm, and the tap density is 3.0 to 7 g / cm3 The average particle size of the microcrystalline silver powder is 0.2 to 2 μm, and the tap density is 1 to 3g / cm3 .
3. The silver conductive paste according to claim 1, characterized in that The organic carrier and the organic solvent in the hydrogenated rosin ester solution are the same.
4. The silver conductive paste according to claim 1, characterized in that The organic carrier and the hydrogenated rosin ester solution are prepared separately, or prepared by adding resin and hydrogenated rosin ester into the same solvent system according to a certain ratio.
5. A method for preparing a silver conductor paste, for preparing the silver conductor paste according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps:
1. Preparation of glass powder, organic carrier and hydrogenated rosin ester solution Preparation of glass powder: weigh the oxides in proportion to the composition of the glass powder, mix them thoroughly, and evenly melt them at 1000-1200°C, quench the evenly melted glass to obtain coarse glass particles, and centrifugally ball-mill the coarse glass particles to obtain powder with an average particle size of 0.2-2 μm, and then dry them to obtain glass powder; Preparation of organic carrier: Heat the organic solvent to 60-90°C, add the resin in sequence under stirring, continue stirring until dissolved, and finally form a transparent homogeneous solution to obtain the organic carrier; Preparation of hydrogenated rosin ester solution: heat the organic solvent to 60-90°C, add hydrogenated rosin ester in sequence under stirring, continue stirring until dissolved, and finally form a transparent homogeneous solution to obtain hydrogenated rosin ester solution; (ii) Preparation of silver conductor paste: the organic carrier prepared above, the hydrogenated rosin ester solution prepared above, the spherical silver powder, the flaky silver powder, the microcrystalline silver powder, the glass powder prepared above, the high-temperature wetting agent, and part of the organic diluent are mixed according to the formula ratio of the silver conductor paste product according to claim 1, and after being mixed evenly, they are fully ground and rolled. The semi-finished product after rolling is added with the remaining organic diluent to adjust the viscosity to a suitable value, filtered, and then packaged to obtain the silver conductor paste; or, the organic carrier prepared above, the hydrogenated rosin ester solution prepared above, the spherical silver powder, the flaky silver powder, the microcrystalline silver powder, the glass powder prepared above, and the high-temperature wetting agent are mixed according to the formula ratio of the silver conductor paste product described above, and after being mixed evenly, they are fully ground and rolled. The semi-finished product after rolling is added with the organic diluent to adjust the viscosity to a suitable value, filtered, and then packaged to obtain the silver conductor paste.
6. The method for preparing the silver conductive paste according to claim 5, characterized in that: The preparation of the organic carrier and the preparation of the hydrogenated rosin ester solution are replaced by adding the resin and the hydrogenated rosin ester into the same solvent system for preparation.
Citation Information
Patent Citations
Method for preparing colorless hydrogenated rosin ester resin
CN102002321A
Conductive paste composition and method of manufacturing multilayer ceramic capacitor using the same
CN102117671A
Preparation method of water-based rosin resin tackifying emulsion
CN102911376A
Washing chip solid crystal solder paste and preparing method thereof
CN105855749A
Low-silver content high-adhesion back silver paste for PERC (passivated emitter and rear cell) and preparation method of low-silver high-adhesion back silver paste