A device and method for forming large-size casting glass with few bubbles and uniform texture

By designing a flow platform structure with tapering width and upward slope in the glass forming device, the problem of uneven texture and bubbles in the thick glass plate is solved, efficient bubble removal and texture uniformity are achieved, and the heat resistance of the product is improved. Impact performance, suitable for large-scale mass production.

CN116589169BActive Publication Date: 2024-10-11CHINA CONSTR FOURTH ENG DIV CORP LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310366804.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-11
Estimated Expiration
2043-04-06

AI Technical Summary

Technical Problem

The existing glazed thick plate stacking and firing process results in uneven texture and the existence of bubbles, and poor thermal shock resistance, making it difficult to adapt to the requirements of large-scale mass production.

Method used

A device for forming large-sized cast glass with less bubbles and uniform texture is designed, including a melting device, a flow tube and a flow platform. The bottom surface of the flow platform is an inclined lip brick structure with tapering width and upward slope to reduce bubbles. Form and promote the secondary mixing of the glass liquid to ensure that the bubbles are discharged and the glass liquid flows evenly during the flow process.

Benefits of technology

It effectively eliminates the problems of bubbles and uneven mixing in the glaze firing process. The product has low bubble rate, good uniformity, and a thermal shock resistance temperature difference of more than 50°C, making it suitable for large-scale mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116589169B_ABST
    Figure CN116589169B_ABST
Patent Text Reader

Abstract

The present invention discloses a large-size casting glass molding device and method with less bubbles and uniform texture. The molding device includes a melting device, a flow pipe, a flow platform and a molding mold for receiving the glass liquid flowing out of the flow platform; the flow pipe connects the melting device and the flow platform; the outlet section of the glass liquid on the bottom of the flow platform is an inclined lip brick with a gradually decreasing width and tilted upward along the direction of the glass liquid flowing out; the side surface of the inclined lip brick at one end of the glass liquid outlet is arc-shaped. The molding method adopts the molding device, including: putting the blank into the melting device, heating it to 400-900℃ and keeping it warm for 0.5-1h, continuing to heat the blank to 700-1250℃ to melt, and obtaining flowing glass liquid; the glass liquid overflows to the flow platform through the flow pipe, flows out along the inclined lip brick and enters the molding mold for molding; the molded glass is cooled to 450-630℃ for annealing, and the temperature is reduced to below 45℃ at a rate of less than 20℃ / h, and demolding to obtain large-size casting glass.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of colored glaze production, and in particular to a device and method for forming large-size casting colored glaze with few bubbles and uniform texture. Background Art

[0002] Colored glaze has the characteristics of flowing light and ever-changing magnificence. Since ancient times, it has been an important decorative component in traditional Chinese architecture and is usually used in important buildings such as palaces, temples, and tombs.

[0003] In recent years, large and thick glazed plates have become a favorite of designers for architectural decoration, which places higher demands on the appearance and quality of glazed plates.

[0004] Thick glass sheets are typically produced using a stacking process. Stacking involves stacking glass blanks in a mold in a specific arrangement within a furnace, then raising the furnace temperature to melt and shape the glass blanks. Due to the low fluidity of the melted glass blanks during stacking, insufficient mixing with the surrounding glass blanks results in uneven texture after forming, with noticeable seams visible when observed under a stress meter. Furthermore, during stacking, a small amount of air remains between the melted glass blanks, which cannot be eliminated and remains in the glass sheet, forming distinct bubble clusters or large bubbles.

[0005] The uneven texture and the presence of bubbles make the stacked large-plate glass have poor resistance to thermal shock. It will generally break when the temperature difference is 30°C, and it is easy to break when used outdoors in extreme weather.

[0006] Patent specifications with publication numbers CN 103466946 A and CN 103466947 A disclose a process for preparing high-quality colored glass with good clarification effect. Improvements are made from the raw material perspective, using cerium dioxide and antimony trioxide in combination as clarifiers. The clarification effect is significantly better than using only cerium dioxide or antimony trioxide. By controlling the ratio of cerium dioxide to antimony trioxide within the range of 1:(2-4), the prepared colored glass has good gloss and few bubbles.

[0007] Patent specification CN 114920447 A discloses a method for preparing, molding, and producing a low-bubble borosilicate glass. The patent utilizes a specific guide tube design to direct the molten glass from the melt into the molding device. The overflow outlet at the tail of the guide tube significantly reduces the formation of secondary bubbles during the glass drainage process. Furthermore, the temperature of the outlet section at the tail of the guide tube is controlled to regulate the thickness of the flow layer at the overflow section. A higher outlet temperature can reduce the thickness of the glass layer and more thoroughly expel bubbles. This patented technology adjusts the temperature in real time based on the flow state of the glass liquid, requiring precise temperature zone distribution and control. While this technology can minimize bubbles when used for single-product production, it places high demands on practical operation and control, making it challenging to implement in large-scale batch production. Summary of the Invention

[0008] The present invention provides a large-size casting glass molding device with few bubbles and uniform texture, which solves the problem of uneven texture and many bubbles in the stacking of thick glass plates. The molding can be performed in only one temperature zone or temperature without increasing the original operation control difficulty, and is suitable for large-scale batch production.

[0009] The specific technical solutions are as follows:

[0010] A large-sized casting glass molding device with few bubbles and uniform texture comprises a melting device, a flow pipe, a flow platform, and a molding die for receiving the glass liquid flowing out of the flow platform;

[0011] The flow pipe connects the melting device and the flow platform;

[0012] The outlet section of the glass liquid on the bottom of the flow platform is an inclined lip brick with a gradually decreasing width and an upward inclination along the outflow direction of the glass liquid; the inclined lip brick is located at one end of the glass liquid outlet and has an arc-shaped side. The arc design has a smooth surface, which can prevent the glass liquid from being entrained in air during the casting process and reduce bubbles.

[0013] The width of the outlet section of the glass liquid on the bottom surface of the flow platform is gradually reduced, so that the glass liquid can be gathered to the middle, thereby promoting the secondary mixing of the glass liquid.

[0014] The outlet section of the glass liquid on the bottom surface of the flow platform is inclined upward, which is conducive to the discharge of bubbles during the flow of the glass liquid.

[0015] The present invention adds a flow platform with a specific structure, thins the glass liquid at the outlet of the flow platform, and adds a bubble discharge. At the same time, the glass liquid undergoes secondary mixing during the flow process on the flow platform, making the final glass product more uniform in texture.

[0016] The molding device designed by the present invention can effectively eliminate the problems of bubbles and uneven mixing caused by the glass stacking and firing process. The product has a low bubble rate and good uniformity. Its strength is better than that of large-plate glass produced by the stacking and firing process. It can withstand heat shock temperature differences of more than 50°C, can withstand drastic temperature changes, and meet the requirements of outdoor use.

[0017] The melting device refers to a device that can melt the glass blank into glass liquid and transfer the glass liquid to the flow platform through the flow pipe.

[0018] The cross-sectional area of ​​the flow tube can be calculated by computational fluid dynamics methods based on product quality, glass viscosity, molding temperature, molding time, etc.

[0019] In a preferred example, the large-size casting glass molding device with few bubbles and uniform texture has one end of a flow tube connected to the bottom surface of the melting device, and the other end passes through the bottom surface of the flow platform from bottom to top, so that the glass liquid from the melting device overflows from the other end of the flow tube into the flow platform, and the overflow process can effectively release bubbles.

[0020] In a preferred embodiment, the large-size casting glass forming device with few bubbles and uniform texture has a U-shaped flow pipe with no horizontal section or right-angle section at the bottom, which reduces the flow pressure of the glass liquid.

[0021] In a preferred embodiment, in the large-size casting glass forming device with few bubbles and uniform texture, the nozzle at the other end of the flow pipe is 50 to 100 mm higher than the inner bottom surface of the flow platform.

[0022] In a preferred embodiment, in the large-sized casting glass forming device with few bubbles and uniform texture, the bottom surface of the melting device is 100 to 200 mm higher than the inner bottom surface of the flow platform.

[0023] In a preferred example, the device for forming large-sized cast glass with fewer bubbles and uniform texture has a height difference between the lowest point and the highest point of the inclined top surface of the inclined lip brick of 30 to 80 mm, and an upward inclination angle of the inclined top surface of the inclined lip brick of 3 to 9°, which can obtain large-sized cast glass with fewer bubbles and more uniform texture.

[0024] In a preferred embodiment, the apparatus for forming large-scale glass castings with low bubbles and uniform texture has a slanted lip brick with a slanted lip width of 1 / 3 to 2 / 3 the width or diameter of the glass product to be produced. If the slanted lip is too wide, the slanted lip will be too thin, potentially preventing some areas from being wetted and resulting in uneven distribution of the glass. If the slanted lip is too narrow, the slanted lip will be too thick, making it difficult to expel bubbles.

[0025] In the large-size casting glass forming device with few bubbles and uniform texture, the glass liquid outflow outlet of the oblique lip brick can be located at one end or the middle position of the forming mold.

[0026] In a preferred embodiment, the large-scale casting glass forming device with few bubbles and uniform texture has three retaining walls on the side of the flow platform and one outlet. The structure is a tapered trapezoid when viewed from above, and the ratio of the width of the widest part of the trapezoid to the narrowest part as the glass liquid flow outlet is 4 / 3 to 3 / 2. Such a design of changing the width ratio can improve the uniformity of the secondary mixing of the glass liquid.

[0027] The present invention can control the flow rate and thickness of the flow material by adjusting the diameter of the flow pipe and the width of the glass liquid outlet of the flow platform.

[0028] In a preferred embodiment, the device for forming large-sized cast glass with few bubbles and uniform texture comprises a melting device, a flow pipe, a flow platform and a forming mold in the same heating furnace, which can be a single temperature zone or a multi-temperature zone.

[0029] In a preferred example, the large-size casting glass molding device with few bubbles and uniform texture maintains the flow platform temperature not lower than the flow pipe temperature, and the flow pipe temperature not lower than the melting device temperature. Such a design can prevent the viscosity of the glass liquid from increasing during the flow process, thereby ensuring good fluidity of the glass liquid.

[0030] The forming mold used in the present invention may have concave-convex patterns or may not have concave-convex patterns.

[0031] The present invention also provides a method for forming large-sized casting colored glass with few bubbles and uniform texture, and adopts the device for forming large-sized casting colored glass with few bubbles and uniform texture;

[0032] The method for forming large-sized cast glass with few bubbles and uniform texture specifically comprises the following steps:

[0033] S1. Place the blank into a melting device and heat it to 400-900°C for 0.5-1h, then continue heating the blank to 700-1250°C to melt and obtain flowing glass liquid;

[0034] S2, the glazing liquid overflows through the flow pipe to the flow platform, flows out along the oblique lip brick and enters the forming mold for forming;

[0035] S3. Cool the formed colored glass to 450-630° C. for annealing, slowly cool it to below 45° C. at a rate of less than 20° C. / h, and demold it to obtain a large-sized cast colored glass.

[0036] The method and device of the present invention are particularly suitable for making large-sized casting glass. In a preferred embodiment, the thickness of the large-sized casting glass is not less than 25 mm, and the plane area is not less than 0.5 m 2 The large-sized cast colored glaze may be a colored glaze plate. The large-sized cast colored glaze may be of uniform thickness or of non-uniform thickness.

[0037] Compared to thick glaze produced by stacking and firing, the method and apparatus of the present invention reduces bubbles by over 50%, achieves uniform stress distribution, and eliminates internal splicing marks. Compared to stacking and firing thick glaze, the molding method and apparatus of the present invention can achieve uniform texture and improve thermal shock resistance by over 15°C.

[0038] Glass casting is a casting process that melts glass raw materials or blanks at a certain temperature and injects them into a mold to form them. When the glass blanks are melted, the gas between the blanks will be enclosed in the molten glass liquid and brought into the mold. After molding, a large number of bubbles will remain in the product, affecting the appearance and mechanical strength of the glass products. At the same time, during the casting process, the short movement distance of the glass liquid after melting and the single movement direction will cause the texture of the entire glass product to be uneven, which will also affect the strength of the glass products. Traditional methods to solve the bubble problem are to increase the temperature and to increase the bubble removal time at high temperature. Increasing the temperature and extending the bubble removal time will increase energy consumption, but neither will effectively solve the problem of unevenness. The present invention can use the device design to allow the glass liquid to flow along the designed route on the basis of keeping the original molding temperature and molding time unchanged, effectively eliminating bubbles, and at the same time, the glass liquid is evenly mixed during the flow process, thereby increasing the strength of the product.

[0039] Compared with the prior art, the present invention has the following beneficial effects: the present invention can obtain a colored glass product with fewer bubbles and more uniform texture without increasing energy and time consumption. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is a schematic structural diagram of a large-sized casting glass forming device with few bubbles and uniform texture according to Example 1;

[0041] Figure 2 This is a schematic diagram of the main structure of the flow platform in Example 1;

[0042] Figure 3 Schematic diagram of the top view of the flow platform in Example 1;

[0043] In the picture:

[0044] 1- Melting device 2- Flow pipe 3- Flow platform

[0045] 4-forming mold 5-heating furnace 6-oblique lip brick. DETAILED DESCRIPTION

[0046] The present invention will be further described below with reference to the accompanying drawings and specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.

[0047] In the following examples, the operating methods without specifying specific conditions are generally carried out under conventional conditions or conditions recommended by the manufacturer.

[0048] Example 1

[0049] like Figure 1 As shown, a large-scale casting glass molding device with few bubbles and uniform texture includes a melter 1, a flow pipe 2, a flow platform 3, and a molding die 4 for receiving the glass liquid flowing from the flow platform 3. The melter 1, flow pipe 2, flow platform 3, and molding die 4 are located in the same heating furnace 5, and the temperature of the flow platform 3 is maintained at no lower than that of the flow pipe 2, and the temperature of the flow pipe 2 is maintained at no lower than that of the melter 1.

[0050] The flow pipe 2 is U-shaped, with no horizontal section or right-angle section at the bottom. The diameter of the flow pipe 2 is 40mm. One end of the flow pipe 2 is connected to the bottom surface of the melting device 1, and the other end passes through the bottom surface of the flow platform 3 from bottom to top. The pipe opening at the other end of the flow pipe 2 is higher than the lowest point of the bottom surface of the flow platform 3 (which can also be considered as the bottom surface of the melting device 1). Figure 2 、 Figure 3 The glass liquid from the melting device 1 overflows from the other end of the flow tube 2 and enters the flow platform 3.

[0051] The bottom surface of the melting device 1 is higher than the lowest point of the bottom surface of the flow platform 3 (which can also be considered as Figure 2 、 Figure 3 Point A in the middle) 160mm.

[0052] like Figure 2 、 Figure 3 As shown, the flow platform 3 has three retaining walls and one outlet. The structure is a tapered trapezoid when viewed from above. The widest part of the trapezoid is 750 mm wide, and the narrowest part, which is the glass liquid outlet, is 550 mm wide.

[0053] The bottom surface of the flow platform 3 corresponding to the other end of the flow tube 2 is a plane, and near the glass liquid outlet section is an inclined lip brick 6 with a gradually decreasing width and an upward inclination along the direction of the glass liquid outflow. The lowest point of the inclined top surface of the inclined lip brick 6 is point A, and the highest point is point B. The height difference between point A and point B is 60 mm. The side surface of the inclined lip brick 6 at one end of the glass liquid outlet (i.e., the end at point B) is arc-shaped. The upward inclination angle of the inclined top surface of the inclined lip brick 6 is 4°. The glass liquid outflow outlet width of the inclined lip brick 6 is 550 mm. The glass liquid outflow outlet of the inclined lip brick 6 is located at one end of the forming mold 4.

[0054] The above-mentioned large-size casting glass molding device with few bubbles and uniform texture is used to carry out a large-size casting glass molding method with few bubbles and uniform texture. The composition of the blank is SiO271%, B2O3 14.3%, Al2O33.1%, BaO 2.1%, CaO 0.9%, Na2O 5%, K2O 3%, TiO2 0.4%, and ZnO 0.2% by mass percentage.

[0055] According to the temperature-viscosity curve of the blank, the molding temperature is calculated to be 1100℃. The large-size casting glass to be produced is a thick plate glass with dimensions of 2500mm×1000mm in length and width, a thickness variation of 30 to 140mm, and a total weight of 500kg.

[0056] The specific steps of the glass forming method for large-sized castings with few bubbles and uniform texture include:

[0057] 1) Place the blank into the melting device 1 and heat it to 890°C and keep it warm for 1 hour;

[0058] 2) After keeping warm, continue heating the blank to 1100℃ to melt and obtain flowing glass liquid;

[0059] 3) The molten glass liquid overflows through the flow pipe 2 to the flow platform 3;

[0060] 4) The glass liquid enters the flow platform 3, and the slope of the flow platform 3 is controlled to make the glass liquid flow into the mold 4 with a certain thickness and uniformity;

[0061] 5) The formed glass is cooled to 560°C for annealing, and then slowly cooled to below 45°C at a rate of less than 20°C / h, and then taken out of the furnace to obtain thick plate glass.

[0062] In this embodiment, the bubble diameter of the thick plate glass product is 0.1 to 1 mm, the number of bubbles is 15 per square meter, the stress distribution is uniform, there are no splicing marks inside, and the thermal shock resistance is 52°C.

[0063] Comparative Example 1

[0064] The difference from Example 1 is that: the traditional stacking firing process is adopted, the blanks are stacked in the mold, kept at 890℃ for 1h, melted and formed at 1100℃, the formed glass is cooled to 560℃ for annealing, and slowly cooled to below 45℃ at a rate of less than 20℃ / h, and then taken out of the furnace to obtain thick plate glass.

[0065] The diameter of the bubbles in the thick plate glass of this comparative example is 0.1-1 mm, the number of bubbles is 52 per square meter, the internal splicing is obvious when observed under a polarizing microscope, and the thermal shock resistance is 35℃.

[0066] Example 2

[0067] A large-scale casting glass forming device with few bubbles and uniform texture similar to Example 1 is used, except that the diameter of the flow pipe 2 is 36 mm, the nozzle at the other end of the flow pipe 2 is 70 mm higher than the lowest point of the inner bottom surface of the flow platform 3, the width of the widest part of the trapezoid of the flow platform 3 is 700 mm, the width of the narrowest part of the glass liquid flow outlet (that is, the width of the glass liquid flow outlet of the inclined lip brick 6) is 480 mm, and the upward inclination angle of the inclined top surface of the inclined lip brick 6 is 3°.

[0068] The above-mentioned large-size casting glass molding device with few bubbles and uniform texture is used to carry out a large-size casting glass molding method with few bubbles and uniform texture. The blank composition, by mass percentage, is SiO272%, B2O3 2%, Al2O3 3.1%, CaO 3%, Na2O 11%, K2O 5%, TiO2 0.5%, ZnO 0.4%, and MgO 3%.

[0069] According to the temperature-viscosity curve of the blank, the molding temperature is calculated to be 1060°C. The large-sized casting glass to be produced is a thick plate glass with dimensions of 2500mm×1000mm in length×width, 90mm in thickness, and a total weight of 460kg.

[0070] The specific steps of the glass forming method for large-sized castings with few bubbles and uniform texture include:

[0071] 1) Place the blank into the melting device 1 and heat it to 830°C and keep it warm for 1 hour;

[0072] 2) After keeping warm, continue heating the blank to 1060℃ to melt and obtain flowing glass liquid;

[0073] 3) The molten glass liquid overflows to the flow platform 3 through the flow pipe 2;

[0074] 4) The glass liquid enters the flow platform 3, and the slope of the flow platform 3 is controlled to make the glass liquid flow into the mold 4 with a certain thickness and uniformity;

[0075] 5) The formed glass is cooled to 527°C for annealing, and then slowly cooled to below 45°C at a rate of less than 20°C / h, and then taken out of the furnace to obtain thick plate glass.

[0076] In this embodiment, the bubble diameter of the thick plate glass product is 0.1 to 1 mm, the number of bubbles is 12 per square meter, the stress distribution is uniform, there are no splicing marks inside, and the thermal shock resistance is 54°C.

[0077] Comparative Example 2

[0078] The difference from Example 2 is that: the traditional stacking firing process is adopted, the blanks are stacked in the mold, kept at 830°C for 1 hour, melted and formed at 1060°C, the formed glass is cooled to 527°C for annealing, and slowly cooled to below 45°C at a rate of less than 20°C / h, and then taken out of the furnace to obtain thick plate glass.

[0079] The diameter of the bubbles in the thick plate glass of this comparative example is 0.1 to 1 mm, the number of bubbles is 46 per square meter, the internal splicing is obvious when observed under a polarizing microscope, and the thermal shock resistance is 36°C.

[0080] In addition, it should be understood that after reading the above description of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. A large-size casting glass forming device with few bubbles and uniform texture, characterized in that: It comprises a melting device (1), a material flow pipe (2), a material flow platform (3), and a molding mold (4) for receiving the glass liquid flowing out of the material flow platform (3); The flow pipe (2) connects the melting device (1) and the flow platform (3); one end of the flow pipe (2) is connected to the bottom surface of the melting device (1), and the other end passes through the bottom surface of the flow platform (3) from bottom to top, so that the glass liquid from the melting device (1) overflows from the other end of the flow pipe (2) and enters the flow platform (3); the flow pipe (2) is U-shaped, and has no horizontal section or right-angle section at the bottom; The outlet section of the glass liquid on the bottom surface of the flow platform (3) is an inclined lip brick (6) with a gradually decreasing width and inclined upward along the direction of the glass liquid outflow; the side surface of the inclined lip brick (6) at one end of the glass liquid outlet is arc-shaped; the height difference between the lowest point and the highest point of the inclined top surface of the inclined lip brick (6) is 30-80 mm; the upward inclination angle of the inclined top surface of the inclined lip brick (6) is 3-9°; the width of the glass liquid outlet of the inclined lip brick (6) is 1 / 3-2 / 3 of the width or diameter of the glass product to be manufactured; the side surface of the flow platform (3) has three retaining walls and one outlet, and the structure is a gradually decreasing trapezoid when viewed from above, and the ratio of the width of the widest part of the trapezoid to the narrowest part as the glass liquid outlet is 4 / 3-3 / 2.

2. The large-size casting glass forming device with few bubbles and uniform texture according to claim 1 is characterized in that: The pipe opening at the other end of the material flow pipe (2) is 50 to 100 mm higher than the inner bottom surface of the material flow platform (3); The bottom surface of the melting device (1) is 100 to 200 mm higher than the inner bottom surface of the material flow platform (3).

3. The large-size casting glass forming device with few bubbles and uniform texture according to claim 1 is characterized in that: The glass liquid outflow outlet of the oblique lip brick (6) is located at one end or the middle of the forming mold (4).

4. The large-size casting glass forming device with few bubbles and uniform texture according to claim 1 is characterized in that: The melting device (1), the material flow pipe (2), the material flow platform (3) and the forming mold (4) are in the same heating furnace (5); The temperature of the material flow platform (3) is maintained not lower than the temperature of the material flow pipe (2), and the temperature of the material flow pipe (2) is maintained not lower than the temperature of the melting device (1).

5. A method for forming large-sized cast glass with few bubbles and uniform texture, characterized in that: A large-size casting glass forming device with few bubbles and uniform texture as described in any one of claims 1 to 4 is used; The method for forming large-sized cast glass with few bubbles and uniform texture specifically comprises the following steps: S1, placing the blank into a melting device (1) and heating it to 400-900°C for 0.5-1h, then continuing to heat the blank to 700-1250°C to melt it and obtain flowing glass liquid; S2, the glass liquid overflows through the flow pipe (2) to the flow platform (3), flows out along the inclined lip brick (6) and enters the forming mold (4) for forming; S3, cooling the formed colored glaze to 450-630°C for annealing, slowly cooling to below 45°C at a rate of less than 20°C / h, and demolding to obtain a large-sized cast colored glaze.

6. The method for forming large-sized casting colored glass with few bubbles and uniform texture according to claim 5, characterized in that: The thickness of the large-sized casting glass is not less than 25mm, and the plane area is not less than 0.5m 2 .