A composite method of shear thickening fluid and fabric

By adding ammonia water to the shear thickening fluid and combining it with ultrasonic treatment technology, the problem of solvent and nanoparticle separation in the shear thickening fluid and fabric composite is solved, significantly improving the strength and puncture resistance of the composite material, and achieving high efficiency Preparation of nanocomposites.

CN116590911BActive Publication Date: 2024-10-15ZHONGSHAN LAIPU NEW MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310499970.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-06
Publication Date
2024-10-15
Estimated Expiration
2043-05-06

AI Technical Summary

Technical Problem

In the existing composite method of shear thickening fluid and fabric, the solvent and nanoparticles of the fluid are easily separated, resulting in poor composite effect and poor puncture resistance.

Method used

By adding ammonia water with a pH of 7.1 to 9 to the shear thickening fluid for premixing, and then using medium-frequency ultrasound in a water bath for dispersion, combined with high-frequency ultrasound during the impregnation process to ensure uniform dispersion of nanoparticles and bubbles within the fabric Removed to form high-strength, high-performance composite materials.

Benefits of technology

It achieves the uniform dispersion of shear thickening fluid in the fabric, significantly improves the strength and puncture resistance of the composite material, avoids the introduction of external impurities, and improves the mechanical properties of the composite material through the green dilution process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116590911B_ABST
    Figure CN116590911B_ABST
Patent Text Reader

Abstract

The present invention discloses a composite method of a shear thickening fluid and a fabric, comprising the following steps: adding ammonia water with a pH value of 7.1 to 9 to the shear thickening fluid, mixing to obtain a premixed liquid, the prepared premixed liquid is milky white and has clusters of agglomerated millimeter and micrometer particles; placing the premixed liquid in a closed container, and dispersing it by medium-frequency ultrasound in a water bath to obtain a uniform dilution; immersing the fabric in the dilution, performing high-frequency ultrasound treatment during the immersion process, squeezing out excess liquid after immersion, and drying the fabric. The present invention does not introduce external impurities when dispersing the fluid, uses medium-frequency ultrasound treatment to prevent particle agglomeration, and is supplemented by high-frequency ultrasonic oscillation during immersion, which can eliminate micrometer-level and submicrometer-level bubbles in the fabric structure, increase the composite uniformity of the fluid and the fabric, and increase the strength and puncture-proof performance of the composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a composite method of a shear thickening fluid and a fabric, belonging to the technical field of application of shear thickening fluid composite materials. Background Art

[0002] Shear thickening fluid is a liquid material that is very sensitive to stress. It is composed of nanoparticles and solvent. When subjected to external stress, the nanoparticles in the fluid can instantly aggregate to form particle clusters, causing the concentration of the fluid to increase sharply and then exhibit solid-like properties to resist external forces. This characteristic makes shear thickening fluid have a wide range of application prospects in the field of protection.

[0003] Shear thickening fluid can be applied to fabrics to make fully flexible bulletproof and stab-proof composites, which have broad application prospects. There are two commonly used composite processes: 1) The fluid is directly coated on the surface of the fabric, and it is slowly infiltrated into the fabric by hot pressing to form a composite; 2) The fluid is diluted with volatile solvents such as methanol and ethanol, and then the fabric is impregnated and taken out and dried to obtain a composite. Although both methods can produce composites, the composite effect and stab-proof performance are defective. Method 1 causes the solvent and nanoparticles of the fluid to separate, the solvent is absorbed into the fabric, and the particles agglomerate and deposit on the surface of the fabric, resulting in poor composite effect. The composite obtained by method 2 has low strength and has basically no stab-proof effect on GA68~2019 standard D1 blades. Therefore, a method for preparing high-strength and high-performance composites is needed. Summary of the invention

[0004] The purpose of the present invention is to solve the problems in the prior art that the shear thickening fluid composite fabric has poor effect and poor puncture resistance, and to provide a composite method of a shear thickening fluid and a fabric, which can evenly disperse the shear thickening fluid into the fabric and improve the strength and puncture resistance of the composite fabric.

[0005] The objective of the present invention is achieved through the following technical solutions:

[0006] A method for compounding a shear thickening fluid and a fabric, characterized by comprising the following steps:

[0007] a. Premixing: Add ammonia water with a pH of 7.1 to 9 to the shear thickening fluid and mix well to obtain a premixed liquid. The prepared premixed liquid is milky white and has clusters of millimeter and micrometer-sized particles;

[0008] b. Dispersion: Place the premixed solution in a sealed container and disperse it by medium-frequency ultrasound in a water bath to obtain a uniform diluted solution;

[0009] c. Impregnation: Immerse the fabric in the diluent and perform high-frequency ultrasonic treatment during the impregnation process. After impregnation, squeeze out the excess liquid and dry the fabric.

[0010] During the premixing process of the present invention, the mass ratio of the fluid to the ammonia water is 1:0.5-3. The ammonia water can make the surface of the silicon dioxide particles negatively charged, so that the particles are dispersed by charge repulsion, and agglomeration is effectively avoided. In addition, the ammonia water can be completely removed by drying, and impurities that affect the rigid collision of the nanoparticles will not be introduced into the fluid, thereby avoiding affecting the mechanical properties of the final composite material.

[0011] During the dispersion process of step b, the ultrasonic power density is 50-100 W / gallon, the ultrasonic frequency is 30-40 kHzf, the ultrasonic temperature is 30-50°C, and the ultrasonic time is 10-30 min. Although low-frequency ultrasonic waves (20-28 kHz) have a strong cavitation effect, they can cause local overheating of the liquid, which can cause particle agglomeration and precipitation. Water bath ultrasound with an ultrasonic frequency of 30-40 kHz can be used for uninterrupted ultrasonic treatment and is easy to accurately control temperature. The treated dilution is filtered through filter paper with a pore size of 1-3 μm and no residue is found on the surface of the filter paper.

[0012] The dispersed dilution solution does not produce precipitation after standing for 4 days, and separates into layers after standing for 2 to 3 weeks, i.e., the bottom layer is milky white sediment and the upper layer is clear liquid. However, repeating steps 2 and 3 can re-obtain a dilution solution with good uniformity.

[0013] In the impregnation process of step c of the present invention, the ultrasonic power density is 50-100 W / gallon, the ultrasonic frequency is 68-80 kHzf, and the ultrasonic treatment time is 10-30 seconds. The use of high-frequency ultrasonic waves can effectively remove microbubbles in the fabric during the impregnation, making the composite more uniform, and can further disperse the possible micro-particle clusters, thereby increasing the mechanical properties of the composite material.

[0014] Compared with the traditional method, the advantages of the present invention are:

[0015] 1. During the dilution process, the fluid is in a closed container and no external impurities will be introduced.

[0016] 2. Dilution uses medium frequency ultrasonic treatment. Ultrasonic waves in this frequency band can quickly dilute the fluid and will not cause particle agglomeration due to excessive cavitation.

[0017] 3. High-frequency ultrasonic oscillation is used during impregnation to eliminate micron-level and submicron-level bubbles in the fabric structure, increase the composite uniformity of the fluid and the fabric, and increase the strength and puncture-proof performance of the composite material.

[0018] 4. Water bath ultrasound is easy to accurately control temperature because water has a large specific heat capacity and can absorb the heat generated by ultrasound without rapidly heating up. Therefore, the temperature can be accurately controlled without the need for additional cooling devices.

[0019] 5. The dilution process is clean and green, without toxic reagents. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a demonstration diagram of a single yarn pulling experiment;

[0021] Figure 2 The relationship between the pulling force of a single yarn and the pulling displacement of the composite material in Example 1 is shown;

[0022] Figure 3 The relationship between the pulling force of a single yarn and the pulling displacement of the composite material in Example 2 is shown;

[0023] Figure 4 The relationship between the pulling force of a single yarn and the pulling displacement of the composite material in Example 3 is shown;

[0024] Figure 5 The relationship between the pulling force of a single yarn and the pulling displacement of the composite material of Example 4 is shown;

[0025] Figure 6 The relationship between the pulling force of a single yarn of the fabric in comparative example 1 and the pulling displacement;

[0026] Figure 7 The relationship between the pulling force of a single yarn of the fabric of comparative example 2 and the pulling displacement;

[0027] Figure 8 The relationship between the pulling force of a single yarn of the fabric of comparative example 3 and the pulling displacement;

[0028] Fig. 9 This is the relationship between the pulling force of a single yarn of the fabric in comparative example 4 and the pulling displacement. DETAILED DESCRIPTION

[0029] A method for compounding a shear thickening fluid and a fabric, characterized by comprising the following steps:

[0030] a. Premixing: Add ammonia water with a pH value of 7.1 to 9 to the shear thickening fluid, with the mass ratio of fluid to ammonia water being 1:0.5 to 3, and mix well to obtain a pre-milky white mixed solution;

[0031] b. Dispersion: Place the premixed liquid in a sealed container, in a water bath, and ultrasonically disperse it for 10 to 30 minutes at an ultrasonic power density of 50 to 100 W / gallon, an ultrasonic frequency of 30 to 40 kHzf, and an ultrasonic temperature of 30 to 50°C to obtain a uniform dilution solution that passes through a filter paper with a pore size of 1 to 3 μm and has no residual particulate matter;

[0032] c. Immersing: Immerse the fabric in the diluent, and simultaneously perform ultrasonic treatment at a high frequency of 68 to 80 kHz for 10 to 30 seconds, squeeze out excess liquid after immersion, and dry the fabric. The present invention is further described in detail below in conjunction with specific embodiments.

[0033] Embodiment 1:

[0034] Polydisperse silica spheres with diameters of 86 nm to 117 nm were dispersed in polyethylene glycol 300 to obtain a shear thickening fluid with a silica sphere volume fraction of 0.48.

[0035] The fabric is aramid woven fabric, and the composite method of the shear thickening fluid and the fabric is:

[0036] a. Premixing: Add ammonia water with a pH value of 8.5 to the shear thickening fluid, with the fluid and ammonia water mass ratio being 1:1, and mix well to obtain a pre-milky white mixed liquid;

[0037] b. Dispersion: Place the premixed liquid in a sealed container, in a water bath, and ultrasonically disperse it for 20 minutes at an ultrasonic power density of 93W / gallon, an ultrasonic frequency of 40kHzf, and an ultrasonic temperature of 35±2℃ to obtain a uniform diluted liquid. Pass the diluted liquid through a 1μm filter paper, and no particles are found on the filter paper.

[0038] c. Impregnation: immerse the aramid woven fabric in the diluent, and treat it with ultrasound at a high frequency of 75kHzf and an ultrasonic temperature of 35±2℃ for 30s during the impregnation process. After impregnation, extrude it through a pressure roller with a roller pressure of 0.2MPa, squeeze out the excess liquid, and dry the fabric at 80℃ for 30 minutes to obtain a nanocomposite material.

[0039] The strength of nanocomposites is mainly determined by the "single yarn extraction" test. The nanocomposites are cut into 20cm x 12cm rectangles, and a portion of the weft yarn is removed and fixed on a tensile machine. Figure 1 A single warp yarn is fixed on a fixture and pulled out along the warp direction at a uniform speed of 100 mm / min. The range of the tensile testing machine sensor head is 300 N. The induced force during the pulling process is recorded on the computer and displayed as the relationship between the pulling force and the pulling displacement. The results are shown in Figure 2 shown.

[0040] Embodiment 2:

[0041] The shear thickening fluid and the woven fabric are the same as in Example 1, and the compounding method is as follows:

[0042] a. Premixing: Take an appropriate amount of fluid and place it in a wide-mouth bottle, add an equal amount of water with a pH value of 7.1, and prepare a uniform dilution according to steps a and b of the embodiment. Let it stand for 15 days to allow the dilution to separate into layers, with the upper layer being a slightly yellow clear liquid and the lower layer being a milky white sediment;

[0043] b. Dispersion: Place the wide-mouth bottle containing the layered dilution in a water bath, and ultrasonically disperse for 30 minutes at an ultrasonic power density of 52W / gallon, an ultrasonic frequency of 30kHzf, and an ultrasonic temperature of 50±1℃ to obtain a uniform dilution. Pass the dilution through filter paper, and no particles are found on the filter paper.

[0044] c. Impregnation: immerse the aramid woven fabric in the diluent, and simultaneously treat it with ultrasound at a high frequency of 80kHzf and an ultrasonic temperature of 50±1℃ for 30s during the impregnation process. After impregnation, extrude it through a pressure roller with a roller pressure of 0.2MPa, squeeze out the excess liquid, and dry the fabric at 80℃ for 30 minutes to obtain a nanocomposite material.

[0045] The warp yarn extraction force was tested according to the method of Example 1, and the results are as follows: Figure 3 shown.

[0046] Embodiment 3:

[0047] The shear thickening fluid is a high concentration suspension of nano-silica spheres (diameter 500±25nm) in polypropylene glycol, where the volume fraction of the silica spheres is The fabric is a mixed plain woven fabric of ultra-high molecular weight polyethylene and aramid, in which aramid is used in the warp direction and ultra-high molecular weight polyethylene is used in the weft direction. The method for preparing the composite material is as follows:

[0048] a. Premixing: Take an appropriate amount of fluid and place it in a wide-mouth bottle, add ammonia water with a pH value of 9, the mass ratio of fluid to ammonia water is 1:3, and mix well to obtain a milky white premixed solution;

[0049] b. Dispersion: Place the premixed liquid in a sealed container, in a water bath, and ultrasonically disperse it for 10 minutes at an ultrasonic power density of 75W / gallon, an ultrasonic frequency of 35kHzf, and an ultrasonic temperature of 40±1℃ to obtain a uniform diluted liquid. Pass the diluted liquid through filter paper, and no particles are found on the filter paper.

[0050] c. Impregnation: immerse the mixed plain woven fabric in the diluent, and treat it with ultrasound at a high frequency of 68kHzf and an ultrasonic temperature of 42±2℃ for 10s during the impregnation process. After impregnation, extrude it through a pressure roller with a roller pressure of 0.15MPa, squeeze out the excess liquid, and dry the fabric at 80℃ for 30 minutes to obtain a nanocomposite material.

[0051] The warp yarn extraction force was tested according to the method of Example 1, and the results are as follows: Figure 4 shown.

[0052] Embodiment 4:

[0053] The shear thickening fluid is a high concentration suspension of nano-silica spheres (diameter 350±10nm) in polyethylene glycol 300, wherein the volume fraction of the silica spheres is 0.57; the fabric is a plain woven fabric of high-strength polyester. The composite material is prepared by the following method:

[0054] a. Premixing: Take an appropriate amount of fluid and place it in a wide-mouth bottle, add ammonia water with pH = 8.0, so that the mass ratio of fluid to ammonia water is 2:1. Mix well to obtain a milky white premixed liquid;

[0055] b. Dispersion: Place the premixed liquid in a sealed container, in a water bath, and ultrasonically disperse it for 15 minutes at an ultrasonic power density of 50W / gallon, an ultrasonic frequency of 30kHzf, and an ultrasonic temperature of 30°C to obtain a uniform diluted liquid. The diluted liquid was filtered through filter paper, and no granular residue was found on the filter paper;

[0056] c. Impregnation: The polyester fabric is placed in the diluent, and the impregnation process is carried out at a high frequency of 80kHzf and an ultrasonic temperature of 35°C for 20s. After impregnation, it is extruded through a pressure roller with a pressure between rollers of 0.18MPa, and the excess liquid is squeezed out. The fabric is dried at 90°C for 20 minutes to obtain a nanocomposite.

[0057] The warp yarn extraction force was tested according to the method of Example 1, and the results are as follows: Figure 5 shown.

[0058] Comparative Example 1 (direct measurement of extraction force without treatment):

[0059] Without treating the fabric, the warp yarn extraction force was directly tested according to the method of Example 1. The results are as follows: Figure 6 shown.

[0060] Comparative Example 2 (too alkaline water):

[0061] The shear thickening fluid and fabric are the same as those in Example 1. During the premixing process, an equal mass of water with a pH value of ≈ 10 is added. The other steps are the same as those in Example 1 to prepare the nanocomposite material.

[0062] The warp yarn extraction force was tested according to the method of Example 1, and the results are as follows: Figure 7 shown.

[0063] Comparative Example 3 (too acidic water):

[0064] The shear thickening fluid and fabric are the same as those in Example 1. During the premixing process, an equal mass of water with a pH value of 5.3 is added. The other steps are the same as those in Example 1 to prepare the nanocomposite material.

[0065] The warp yarn extraction force was tested according to the method of Example 1, and the results are as follows: Figure 8 shown.

[0066] Comparative Example 4 (no ultrasound, only premixing):

[0067] The shear thickening fluid and fabric are the same as in Example 1, and the compounding method is as follows:

[0068] An appropriate amount of fluid and an equal amount of ammonia water with a pH value of ≈ 8.5 were mixed on a vortex oscillator at a speed of 2500 rpm for 5 hours until a milky white premixed liquid with substantially no stratification was obtained. The nanocomposite material was prepared according to step c of Example 1 without water bath ultrasonic treatment, and the warp yarn extraction force was tested. The results are shown in FIG. Fig. 9 shown.

[0069] Figure 6 It shows that the maximum pull-out force of the untreated aramid woven fabric warp yarn does not exceed 10N. As the warp yarn is slowly pulled out, the pull-out force gradually decreases to 0N. However, for the nanocomposite prepared with ammonia as the diluent, the shear thickening fluid is well attached to the surface of the fabric yarn. The mutual friction between the warp and weft yarns during the pull-out causes the fluid to be stressed and thickened rapidly. Therefore, the maximum pull-out force exceeds 100N, which is more than 10 times the pull-out force of the untreated warp yarn. The pull-out force of a single yarn of the composite material prepared by the traditional preparation method is only 60N.

[0070] The nanocomposite prepared with ammonia water as the diluent, after the warp yarn is pulled to a certain extent, the yarn breaks and the pulling force drops sharply instantly. This is because the nanoparticles of the shear thickening fluid have extremely high hardness. After the fluid thickens, the rigid friction between the particles damages the yarn, so the yarn breaks after being pulled to a certain extent. In addition, the nanocomposite prepared with ammonia water as the diluent exhibits an extremely high pulling force of more than 100N. This is because the ammonia molecules are small in size and have appropriate polarity, which can easily help the fluid fill the micropores of the fabric and make the composite more complete.

[0071] Although the diluted solution prepared by the method of the present invention will cause the nanoparticles to precipitate if left for a long time, a stable mixed solution can be re-formed by repeating the water bath ultrasound step, and the warp yarn extraction force of the prepared composite material will not decrease, which can be proved by comparing the test data of Examples 1 and 2.

[0072] Table 1 is a comparison of the pull-out forces of different fabric types before and after compounding in Example 1, Example 3, and Example 4. The fabric types are divided into aramid, aramid / polyethylene blended fabric, and high-strength polyester fabric. For these three fabrics, the pull-out forces are greatly improved after treatment (at least 10 times), which not only shows that the strength of the composite material prepared by this method is significantly improved, but also shows that this method is applicable to fabrics of various different materials.

[0073] Table 1: Comparison of single yarn pull-out force test before and after different fabric treatments

[0074] Fabric Type Unprocessed After treatment Extraction force increase times Aramid 9.4 100 10.6 Polyethylene / aramid blended 8.2 109 13.3 High-strength polyester 5.3 113 21.3 .

Claims

1. A method for compounding a shear thickening fluid and a fabric, characterized in that The following steps are involved: a. Premixing: Add ammonia water with a pH of 7.1 to 9 to the shear thickening fluid and mix well to obtain a premixed liquid; b. Dispersion: Place the premixed solution in a sealed container and disperse it by medium-frequency ultrasound in a water bath to obtain a uniform diluted solution; c. Impregnation: Immerse the fabric in the diluent and perform high-frequency ultrasonic treatment during the impregnation process. After impregnation, squeeze out the excess liquid and dry the fabric.

2. A method for compounding a shear thickening fluid and a fabric according to claim 1, characterized in that The mass ratio of the fluid to the ammonia water is 1:0.5-3.

3. The method for compounding a shear thickening fluid and a fabric according to claim 1, characterized in that The instrument used for premixing is a vortex shaker.

4. The method for compounding a shear thickening fluid and a fabric according to claim 1, characterized in that The prepared premixed liquid is milky white and has agglomerated clusters of millimeter and micrometer-sized particles.

5. The method for compounding a shear thickening fluid and a fabric according to claim 1, characterized in that During the dispersion process, the ultrasonic power density is 50-100 W / gallon, the ultrasonic frequency is 30-40 kHzf, the ultrasonic temperature is 30-50° C., and the ultrasonic time is 10-30 min.

6. The method for compounding a shear thickening fluid and a fabric according to claim 1, characterized in that During the immersion process, the ultrasonic power density is 50-100 W / gallon, the ultrasonic frequency is 68-80 kHzf, the ultrasonic temperature is 30-40° C., and the ultrasonic treatment time is 10-30 s.

7. The method for compounding a shear thickening fluid and a fabric according to claim 1, characterized in that The diluted solution obtained in step b was left to stand for 4 days without generating precipitation.

8. The method for compounding a shear thickening fluid and a fabric according to claim 1, characterized in that The dilution obtained in step b passes through filter paper with a pore size of 1 to 3 μm and no particulate matter remains.

9. The method for compounding a shear thickening fluid and a fabric according to claim 1, characterized in that The fabric has a liquid content of 7-25% after drying.

Citation Information

Cited By

  • Puncture-resistant and washing-resistant flexible breathable composite material and preparation method thereof

    CN119956608A