Preparation method of tungsten-based alloy material
By spraying atomized droplets of pyrolyzed tungsten-based alloy in a reducing atmosphere in powder metallurgy, the problems of alloy composition segregation and impurities introduction are solved, and the stable performance and excellent comprehensive performance of tungsten-based alloy materials are achieved, which is significantly Improves the microstructure and performance of the material.
Patent Information
- Application Number
- CN202310836717.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-10
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-07-10
AI Technical Summary
When preparing tungsten-based alloy materials by powder metallurgy, due to the difference in size and specific gravity of the metal powder, it is easy to cause segregation of alloy components and introduction of impurities, which affects the performance of the material, resulting in coarse grains and uneven distribution of components, which in turn makes the material performance unstable and comprehensive. Poor performance.
Atomization is performed by adding a reducing agent to a mixed solution containing tungsten and alloy elements to obtain atomized droplets and spray pyrolysis in a reducing atmosphere to obtain a composite powder with uniform components and fine grains. Press-forming and sintering to obtain a tungsten-based alloy material with stable performance and excellent comprehensive performance.
A composite powder with uniform component distribution, fine grains and uniform particle size distribution is achieved, which reduces the sintering temperature and time, optimizes the microstructure, improves the stability and comprehensive performance of the material, and significantly improves the tungsten-based alloy material. performance.
Smart Images

Figure CN116607057B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of powder metallurgy, and in particular to a method for preparing a tungsten-based alloy material. Background Art
[0002] Tungsten-based alloy materials are a type of advanced materials with a variety of applications. Their main component is tungsten, and they usually include other elements such as copper, nickel, and iron. These alloys have excellent properties such as high density, high strength, and high melting point, which makes them have important application value in many fields, such as national defense, electronic products, and aerospace. Tungsten-based alloy materials mainly include high-density alloys and tungsten-copper pseudoalloys. High-density alloys are composed of tungsten, nickel, iron and other elements, and have the characteristics of high density, high strength, and high hardness. They are mainly used in projectiles, aircraft engines and other fields. Tungsten-copper pseudoalloy is composed of two elements, tungsten and copper, and has good thermal conductivity, electrical conductivity and wear resistance. It is an ideal electrode material.
[0003] The preparation methods of tungsten-based alloy materials mainly include powder metallurgy, smelting, etc. Powder metallurgy is one of the most common preparation methods, and its main steps include: mixing, pressing, sintering, etc. of metal powders. First, different types of metal powders are mixed in a predetermined proportion, and then the mixed powders are pressed and formed. Finally, high-temperature sintering is performed to melt the contact points between the metal powders to form a uniform alloy structure. The smelting method is to melt different types of metals together, and then cool and solidify them to form an alloy. This method is suitable for preparing tungsten-based alloy materials with higher purity.
[0004] However, when preparing tungsten-based alloy materials by powder metallurgy, the difference in metal powder size and specific gravity can easily lead to segregation of alloy components and introduce impurities. This will affect the performance of the alloy, such as coarse grains and uneven distribution of components, which will lead to unstable performance of the prepared material and poor overall performance. Summary of the invention
[0005] Based on this, it is necessary to provide a method for preparing a tungsten-based alloy material, which can obtain a tungsten-based alloy material with stable performance and excellent comprehensive performance.
[0006] A method for preparing a tungsten-based alloy material comprises the following steps:
[0007] Providing a mixed solution containing tungsten element and alloy element;
[0008] adding a reducing agent to the mixed solution for atomization to obtain atomized droplets;
[0009] The atomized liquid droplets are sprayed and pyrolyzed in a reducing atmosphere to obtain a composite powder containing tungsten element and alloy element;
[0010] The composite powder is pressed into shape and then sintered to obtain a tungsten-based alloy material.
[0011] In one embodiment, the alloy element includes at least one of iron, nickel and copper.
[0012] In one embodiment, the tungsten element in the mixed solution exists in the form of acid radical ions, and the alloy element in the mixed solution exists in the form of metal cations.
[0013] In one embodiment, the amount of the reducing agent added is ≤ 10% of the volume of the mixed solution.
[0014] In one embodiment, the reducing agent is hydrazine hydrate, sodium cyanide, sodium borohydride or ascorbic acid.
[0015] In one embodiment, the reducing atmosphere comprises a metal oxide reducing gas, and the metal oxide reducing gas is hydrogen or carbon monoxide; the volume content of the metal oxide reducing gas in the reducing atmosphere is ≥5%.
[0016] In one embodiment, the temperature of the spray pyrolysis is 100% to 110% of the decomposition temperature of the component with the highest decomposition temperature in the atomized droplets.
[0017] In one embodiment, the spray pyrolysis time is 0.1 to 10 seconds, and the spray pyrolysis pressure is 3.5 MPa to 6.5 MPa.
[0018] In one embodiment, the pressing pressure is ≥20 MPa.
[0019] In one embodiment, the sintering temperature is 60% to 95% of the conventional sintering temperature, and the sintering time is 1 / 10 to 1 / 2 of the conventional sintering time;
[0020] The conventional sintering temperature and conventional sintering time are the sintering temperature and sintering time required for sintering using the following process:
[0021] Provide tungsten powder and alloy element powder;
[0022] The tungsten powder and the alloy element powder are mixed uniformly according to a certain proportion, and then pressed and sintered in sequence.
[0023] The preparation method of the above-mentioned tungsten-based alloy material is to spray pyrolyze atomized droplets containing tungsten elements, alloy elements and a reducing agent in a reducing atmosphere to obtain a composite powder containing tungsten elements and alloy elements with uniform component distribution, high activity, fine grains and uniform particle size distribution. These composite powders are then pressed into shape and sintered to obtain a tungsten-based alloy material with stable performance and excellent comprehensive performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a SEM image of the tungsten-based alloy material prepared in Example 1;
[0025] Figure 2 This is the SEM image of the tungsten-based alloy material prepared in Example 2. DETAILED DESCRIPTION
[0026] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively below, and preferred embodiments of the present invention are provided. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0028] A method for preparing a tungsten-based alloy material according to one embodiment includes the following steps S110 to S140:
[0029] S110, providing a mixed solution containing tungsten element and alloy element.
[0030] In this embodiment, the alloy element is selected from at least one of iron, nickel and copper.
[0031] It should be noted that the tungsten element in the mixed solution exists in the form of acid ions, such as tungstate, etc. The alloy elements in the mixed solution exist in the form of cations, such as iron ions, nickel ions, copper ions, etc.
[0032] In this embodiment, the mixed solution is prepared by the following method:
[0033] Providing a salt solution containing tungsten element and a salt solution containing alloy elements;
[0034] The above-mentioned mixed solution can be obtained by uniformly mixing the above-mentioned salt solution containing tungsten element and the above-mentioned salt solution containing alloy element in proportion.
[0035] The salt solution containing tungsten element may be an ammonium tungstate aqueous solution, and the salt solution containing alloy elements may be a nickel chloride aqueous solution, a ferric chloride aqueous solution, a cupric chloride aqueous solution, a cupric acetate aqueous solution, or the like.
[0036] It should be noted that the method for preparing the mixed solution is not limited to the one described above. According to the composition of the desired tungsten-based alloy material, any corresponding mixed solution containing tungsten element and alloy element can be provided.
[0037] S120, adding a reducing agent to the mixed solution for atomization to obtain atomized droplets.
[0038] In this embodiment, the amount of the reducing agent added is ≤ 10% of the volume of the mixed solution, wherein the reducing agent is hydrazine hydrate, sodium cyanide, sodium borohydride or ascorbic acid.
[0039] Furthermore, the amount of reducing agent added is 0.5% to 1.0% of the volume of the mixed solution.
[0040] By adding an appropriate amount of reducing agent to the mixed solution for atomization, the raw materials can be reduced under low temperature and liquid phase conditions. Subsequently, the reducing potential can be increased together with the reducing atmosphere to improve the reduction effect, so that the raw materials can be fully reduced in a short time.
[0041] S130, spraying and pyrolyzing the above-mentioned atomized liquid droplets in a reducing atmosphere to obtain a composite powder containing tungsten element and alloy element.
[0042] In this embodiment, the reducing atmosphere includes a metal oxide reducing gas (ie, a gas capable of reducing metal oxides), and the metal oxide reducing gas is hydrogen or carbon monoxide.
[0043] Furthermore, the volume content of the metal oxide reducing gas in the reducing atmosphere is ≥5%; further, the volume content of the metal oxide reducing gas in the reducing atmosphere is 5% to 75%.
[0044] Furthermore, the reducing atmosphere also includes an inert gas, wherein the inert gas is nitrogen or argon.
[0045] Furthermore, the reducing atmosphere is an ammonia decomposition mixed gas, that is, the reducing atmosphere is composed of 75% by volume of hydrogen and 25% by volume of nitrogen.
[0046] The spray pyrolysis time is 0.1 to 10 seconds, and the spray pyrolysis pressure is 3.5 MPa to 6.5 MPa.
[0047] The temperature of the spray pyrolysis is 100% to 110% of the decomposition temperature of the component with the highest decomposition temperature in the atomized droplets. For example, if the component with the highest decomposition temperature in the atomized droplets is ammonium tungstate, and the decomposition temperature of ammonium tungstate is 1000°C, then the temperature of the spray pyrolysis is 1000°C to 1100°C.
[0048] S140, pressing the composite powder into a shape and then sintering it to obtain a tungsten-based alloy material.
[0049] In this embodiment, the pressure of the press forming is ≥ 20 MPa. Further, the pressure of the press forming is 20 MPa to 45 MPa.
[0050] In this embodiment, the sintering temperature is 60% to 95% of the conventional sintering temperature, and the sintering time is 1 / 10 to 1 / 2 of the conventional sintering time.
[0051] It should be noted that the conventional sintering temperature and conventional sintering time mentioned above are the sintering temperature and time of conventional powder metallurgy process, that is, the sintering temperature and time required for the main steps of mixing, pressing and sintering of metal powders. For example, after tungsten powder and alloy element powder are evenly mixed, pressing and sintering are carried out in sequence.
[0052] Compared with first spray pyrolysis to obtain composite oxide powder and then reducing the composite oxide powder, the present application sprays pyrolysis the atomized droplets directly in a reducing atmosphere, which can effectively shorten the process flow and prevent grain growth, thereby obtaining a composite powder with uniform component distribution, fine grains, uniform particle size distribution and high activity, which can effectively reduce the temperature and time required for subsequent sintering, optimize the microstructure, and improve the stability and comprehensive performance of the material.
[0053] It has been verified that the sintering temperature is 60% to 95% of the conventional sintering temperature, and the sintering time is 1 / 10 to 1 / 2 of the conventional sintering time.
[0054] The preparation method of the tungsten-based alloy material can realize the batch, low-cost and continuous production of high-performance tungsten-based alloy materials.
[0055] The following are specific embodiments.
[0056] Example 1
[0057] 1104.66g of ammonium tungstate, 146.73g of nickel chloride and 86.7g of ferric chloride are dissolved in 6.91L, 1.22L and 0.87L of deionized water respectively to prepare corresponding aqueous solutions, and the obtained solutions are fully mixed to obtain a mixed solution, in which the mass ratio of tungsten, nickel and iron is 90:7:3, and then 0.5% of hydrazine hydrate is added to perform ultrasonic atomization, and the obtained atomized droplets are passed into a spray pyrolysis furnace to perform pyrolysis in a reducing atmosphere, wherein the reducing atmosphere is composed of 10% by volume of hydrogen and 90% by volume of nitrogen, the spray pyrolysis temperature is 1000°C (100% of the decomposition temperature of ammonium tungstate with the highest decomposition reduction temperature in the atomized droplets), the spray pyrolysis time is 5 to 6 seconds, and the spray pyrolysis pressure is 3.5MPa. The obtained ultrafine composite powder was pressed into shape at 45MPa and sintered at 1360℃ for 0.5 hours to obtain a tungsten-nickel-iron alloy material with a density of more than 99.5% and a tensile strength of 1020MPa. The microstructure is shown in the figure below. Figure 1shown.
[0058] Example 2
[0059] 547.6g of ammonium tungstate, 55.22g of nickel chloride and 21.16g of cupric chloride were dissolved in 4.56L, 0.46L and 0.18L of deionized water, respectively, to prepare corresponding aqueous solutions, and then the obtained solutions were fully mixed to obtain a mixed solution, wherein the mass ratio of tungsten, nickel and copper in the mixed solution was 93:5:2, and then 1.0% of ascorbic acid was added to perform ultrasonic atomization, and the obtained atomized droplets were passed into a spray pyrolysis furnace to perform pyrolysis in a reducing atmosphere, wherein the reducing atmosphere was composed of 15% by volume of hydrogen and 85% by volume of argon, the temperature of the pyrolysis furnace was 1100°C (110% of the decomposition temperature of ammonium tungstate having the highest decomposition reduction temperature in the atomized droplets), the spray pyrolysis time was 3 to 5 seconds, and the spray pyrolysis pressure was 6.0MPa. The obtained ultrafine composite powder is pressed into shape at 35MPa and sintered at 1320°C for 0.2 hours to obtain a tungsten-nickel-copper alloy material with a density of more than 99.5% and a tensile strength of 938MPa.
[0060] Example 3
[0061] 94.12g of ammonium tungstate and 57.18g of copper acetate were dissolved in 0.588L and 0.476L of deionized water respectively to prepare the corresponding aqueous solution, and then the obtained solution was fully mixed to obtain a mixed solution, in which the mass ratio of tungsten to copper was 80:20, and then 0.5% of hydrazine hydrate was added for ultrasonic atomization, and the obtained atomized droplets were passed into a spray pyrolysis furnace for pyrolysis in a reducing atmosphere, wherein the reducing atmosphere was ammonia decomposition mixed gas, the spray pyrolysis temperature was 1050°C (105% of the decomposition temperature of ammonium tungstate with the highest decomposition reduction temperature in the atomized droplets), the spray pyrolysis time was 8 to 10 seconds, and the spray pyrolysis pressure was 6.5MPa. The obtained ultrafine composite powder was pressed and formed at 45MPa, and sintered at 1360°C for 0.5 hours to obtain a tungsten-copper alloy material with a density of more than 99.5%, with a hardness of 216HB and an electrical conductivity of 33.56%IACS. Figure 2 This is the SEM image of the prepared W-20Cu alloy material.
[0062] Comparative Example 1
[0063] Using traditional powder metallurgy technology, tungsten powder and copper powder with a purity of more than 99.5% and a particle size of 300 mesh are ball-milled and mixed at a mass ratio of 80:20, and then the obtained mixed powder is reduced, pressed and sintered. The obtained ultrafine composite powder is pressed into shape at 50MPa and sintered at 1450℃ for 2 hours to obtain a tungsten-copper alloy material with a density of more than 99.5%, a hardness of 149HB, and an electrical conductivity of 19.33%IACS.
[0064] Comparative Example 2
[0065] 94.12g of ammonium tungstate and 57.18g of copper acetate were dissolved in 0.588L and 0.476L of deionized water, respectively, to prepare corresponding aqueous solutions, and then the obtained solutions were fully mixed to obtain a mixed solution, in which the mass ratio of tungsten to copper in the mixed solution was 80:20, and ultrasonic atomization was performed, and the obtained atomized droplets were passed into a spray pyrolysis furnace, the spray pyrolysis temperature was 1050°C (105% of the decomposition temperature of ammonium tungstate with the highest decomposition reduction temperature in the atomized droplets), the spray pyrolysis time was 8-10 seconds, and the spray pyrolysis pressure was 6.5MPa. The obtained ultrafine composite powder was reduced and cooled in ammonia decomposition mixed gas to obtain a metal composite powder, and then pressed and formed at 50MPa, and sintered at 1450°C for 0.5 hours to obtain a tungsten-copper alloy material with a density of more than 98.1%, and its hardness reached 166HB and its conductivity reached 24.18%IACS.
[0066] Compared with Comparative Example 1, the preparation method of the present application has the characteristics of uniform microstructure and fine grains, which can reduce the sintering temperature, shorten the sintering time, and significantly improve the material performance; and compared with Comparative Example 2, the preparation method of the present application can retain the high specific surface energy activity of the powder through one-step reduction. If the oxide is prepared first, then calcined and reduced, more energy will be consumed during pressing and sintering, increasing the cost, and the surface activity of the powder will be reduced, which is not conducive to sintering, and the performance of the material will also be reduced.
[0067] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a tungsten-based alloy material, characterized in that: The following steps are involved: Providing a mixed solution containing tungsten element and alloy element; adding a reducing agent to the mixed solution for atomization to obtain atomized droplets; The atomized liquid droplets are sprayed and pyrolyzed in a reducing atmosphere to obtain a composite powder containing tungsten element and alloy element; The composite powder is pressed into shape and then sintered to obtain a tungsten-based alloy material; The reducing agent is hydrazine hydrate, sodium cyanide, sodium borohydride or ascorbic acid; The amount of the reducing agent added is 0.5% to 1.0% of the volume of the mixed solution; The reducing atmosphere is composed of a metal oxide reducing gas and an inert gas, wherein the metal oxide reducing gas is hydrogen or carbon monoxide, and the inert gas is nitrogen or argon. The volume content of the metal oxide reducing gas in the reducing atmosphere is 5% to 75%.
2. The method for preparing a tungsten-based alloy material according to claim 1, characterized in that: The alloy element is selected from at least one of iron, nickel and copper.
3. The method for preparing a tungsten-based alloy material according to claim 1 or 2, characterized in that: The tungsten element in the mixed solution exists in the form of acid radical ions, and the alloy element in the mixed solution exists in the form of metal cations.
4. The method for preparing a tungsten-based alloy material according to claim 1, characterized in that: The temperature of the spray pyrolysis is 100% to 110% of the decomposition temperature of the component with the highest decomposition temperature in the atomized droplets.
5. The method for preparing a tungsten-based alloy material according to claim 1, characterized in that: The time of the spray pyrolysis is 0.1 to 10 seconds, and the pressure of the spray pyrolysis is 3.5 MPa to 6.5 MPa.
6. The method for preparing a tungsten-based alloy material according to claim 1, characterized in that: The pressing pressure is ≥20MPa.
7. The method for preparing a tungsten-based alloy material according to claim 1, characterized in that: The sintering temperature is 60% to 95% of the conventional sintering temperature, and the sintering time is 1 / 10 to 1 / 2 of the conventional sintering time; The conventional sintering temperature and conventional sintering time are the sintering temperature and sintering time required for sintering using the following process: Provide tungsten powder and alloy element powder; The tungsten powder and the alloy element powder are mixed uniformly according to a certain proportion, and then pressed and sintered in sequence.