A test calculation method for obtaining high temperature tensile true stress-strain curve

By measuring the immersion liquid on the sample in a high-temperature tensile test, recording the relationship between the solution volume change and the sample drop, fitting to obtain the cross-sectional area function, solving the problem of difficulty in measuring the true stress and strain curve in the prior art, and realizing the Accurate acquisition of the true stress and strain curve during high-temperature tensile process.

CN116609201BActive Publication Date: 2024-12-03ANGANG STEEL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310293341.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-12-03
Estimated Expiration
2043-03-23

AI Technical Summary

Technical Problem

The prior art is difficult to accurately measure the true stress and strain curve of a material in high-temperature tensile tests, especially when the sample deformation is uneven, it is impossible to effectively obtain the cross-sectional area change of the sample, resulting in limitations in stress measurement.

Method used

By stretching the sample with rod-shaped cylinder in the thermal simulation test machine, breaking it into two sections and docking it into a whole, and slowly immersing it in the solution, recording the relationship between the change in the solution volume and the drop distance or time of the sample, Curve fitting obtains a function of the cross-sectional area of ​​the sample, and then calculates the true stress and true strain.

Benefits of technology

It is possible to accurately obtain the cross-sectional area change of the sample regardless of whether the deformation is uniform during high-temperature stretching, and obtain an accurate true stress and strain curve, which overcomes the limitations of the traditional method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116609201B_ABST
    Figure CN116609201B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of thermal simulation test technology, and in particular to a test calculation method for obtaining a high-temperature tensile true stress-strain curve. The present invention establishes a relationship curve between the volume increment caused by the sample being immersed in a solution and the sample's descending distance or the sample's uniform descending time, and finds the relationship between the cross-sectional area of ​​the sample before breaking and the slope of the curve, thereby obtaining the change in the cross-sectional area of ​​the sample during the high-temperature tensile process. Regardless of whether the sample is deformed uniformly during the tensile process, the true stress of the sample during the tensile process can be accurately obtained, thereby obtaining an accurate true stress-strain curve. By analyzing the deformation characteristics of the material, the cross-sectional area of ​​the sample corresponding to the force value during the deformation process is found, so as to effectively obtain the true stress-strain curve of the material during the high-temperature tensile process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermal simulation test, and in particular to a test calculation method for obtaining a high-temperature tensile true stress-strain curve. Background Art

[0002] The plasticity and toughness of materials are important performance parameters that reflect the characteristics of materials. The true stress-strain curve is a true reflection of the plastic deformation law of materials during the tensile process and is an important basis for determining the true destructive strength of materials and their ability to resist deformation.

[0003] At present, thermal simulation test machines and material mechanics test machines are mainly used for high temperature tensile tests, and the high temperature mechanical properties of materials and rolling force prediction are studied based on the high temperature tensile test data. The above test equipment has built-in force sensors, which can directly obtain the force value of the material during the entire test process.

[0004] However, the above equipment is not equipped with a device that can directly obtain the change in the cross-sectional area of ​​the material during the test. During the test, the testing machine can obtain parameters such as the temperature, deformation, force value and stress value of the material through corresponding sensors. For the stress value, one of the important parameters in the high-temperature tensile test data, the equipment can only accurately collect the load force value borne by the sample, and it is difficult to obtain the cross-sectional area of ​​the sample that changes with the stretching process, especially when the sample deforms unevenly during the high-temperature stretching process. It is more difficult to obtain the cross-sectional area of ​​the sample, and stress is the ratio of the load force value to the corresponding cross-sectional area of ​​the sample. Therefore, it is difficult to accurately measure the stress value during the stretching process using existing technology.

[0005] The traditional method of studying the high temperature strength of materials and predicting the rolling force of rolling mills is to obtain the material tensile test data by high temperature tensile method, and then to obtain the stress-strain curve by regression fitting based on this data, and to consider the influence of deformation rate and deformation temperature on rheological stress, so as to obtain a high-precision rolling force prediction value. However, there are always limitations in the measurement of true stress-strain curves; therefore, it is of great significance to develop a method for determining the true stress of tensile tests. Summary of the invention

[0006] In order to overcome the shortcomings of the prior art, the present invention provides a test calculation method for obtaining a high-temperature tensile true stress-strain curve. Regardless of whether the deformation of the sample is uniform during the stretching process, the true stress of the sample during the stretching process can be accurately obtained, thereby obtaining an accurate true stress-strain curve.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A test calculation method for obtaining a high temperature tensile true stress-strain curve, the method specifically comprising the following steps:

[0009] Step 1) A rod-shaped cylindrical simulation sample with a length of L0, mm, is selected, and the simulation sample is heated, kept warm, cooled, and then stretched by a thermal simulation test machine according to a predetermined experimental plan, and the stretching rate is V t , mm / s, until the sample is broken to obtain a sample broken into two sections.

[0010] The two sections of the sample are butted together to form a coaxial whole, and the two sections of the sample are joined by magnetization or adhesion to the state at the moment the sample is stretched and broken.

[0011] Step 2) Take a container filled with sufficient solution, place it on a horizontal surface, and use a solution that does not react with the sample.

[0012] Place the two sections of the sample that have been connected in step 1) perpendicularly to the surface of the solution and slowly place them in the solution in a direction perpendicular to the surface of the solution. During the placement process, two methods can be used: one is to lower the sample by the same distance d, mm each time; the other is to lower the sample at a uniform speed, with a descending speed of v d , mm / s.

[0013] When descending, record the rise of the solution level H, mm; the total volume of the solution and the sample immersed therein V, ml.

[0014] Step 3) Draw a relationship curve between the total volume V, ml of the solution and the sample immersed therein and the sample falling distance d, or draw a relationship curve between the total volume V, ml of the solution and the sample immersed therein and the sample falling time t.

[0015] When the sample is just immersed in the solution, the curve rises straightly. When the table-shaped part of the sample is immersed in the solution, the slope of the curve decreases. When the sample continues to descend to another section, the slope of the curve increases. Finally, the curve rises straightly again.

[0016] Step 4) Perform first-order differentiation on the curve to obtain a curve showing the relationship between the slope of the curve and the sample falling distance d or the slope of the curve and the sample falling time. The slope of the curve corresponds to the volume increment ΔV, ml.

[0017] The maximum value of the curve corresponds to the maximum cross-sectional area of ​​the specimen S1, mm 2 , the minimum value of the curve corresponds to the minimum cross-sectional area of ​​the specimen S2, mm 2 The minimum cross-sectional area at the fracture of the specimen is S2, the distance the specimen drops from the maximum value to the minimum value of the curve is set to Δd, mm, and the time the specimen drops from the maximum value to the minimum value of the curve is set to Δt, s.

[0018] Step 5) Perform polynomial fitting on the portion between the point where the curve starts to drop and the point where the curve drops to the lowest point, and obtain the relationship between the volume increment ΔV and the drop distance or drop time as follows:

[0019] ΔV=f(d) (1)

[0020] ΔV=f(t) (2)

[0021] The maximum value of the curve corresponds to a volume increment of ΔV0, which corresponds to the maximum cross-sectional area S1 of the sample, that is, the original cross-sectional area of ​​the sample. These two parameters are known. Assuming the ratio of the two is K, then

[0022]

[0023] The volume increment ΔV is proportional to the cross-sectional area S of the sample, then

[0024]

[0025] Substituting formula (4) into formula (1) and formula (2), we get

[0026] S=f(d)K (5)

[0027] S=f(t)K (6)

[0028] The function of the cross-sectional area of ​​the specimen within the entire deformation region is established by equations (5) and (6).

[0029] Step 6) Assume that when performing step 1), the time taken for the sample to be stretched from the beginning to a certain length is t1, s, the tensile force value at this time is F1, N, and the time taken for the sample to be stretched from the beginning to being broken is t0, s. If the cross-sectional area of ​​the sample after the stretching time t1 is calculated according to the sample's descending distance, then

[0030]

[0031] Substituting the above formula into formula (5), we get

[0032]

[0033] Among them, Δd, t0, and K are constants that can be measured experimentally;

[0034] If the cross-sectional area of ​​the sample after the sample stretching time t1 is calculated according to the sample falling time, then

[0035]

[0036] Substituting the above formula into formula (6), we get

[0037]

[0038] Among them, Δt, t0, K are constants and can be measured experimentally.

[0039] Formulas (8) and (12) are the relationship between the cross-sectional area of ​​the sample and the stretching time t1 during the stretching process under two methods. The relationship between the tensile force of the sample and the stretching time t1 during the stretching process can be obtained by collecting corresponding data from the testing machine, which is:

[0040] F1=g(t1) (11)

[0041] Then substitute formula (8) and (11) or (10) and (11) into the following formula:

[0042]

[0043] The relationship between the true stress and the stretching time during the deformation process of the sample is obtained.

[0044] Step 7) The relationship between true strain and engineering strain is:

[0045] ε=ln(1+e) (13)

[0046] Where ε is the true strain and e is the engineering strain

[0047] From step 1, the original length of the sample is L0, and the tensile rate is V t , mm / s, then

[0048]

[0049] Substituting formula (14) into formula (13), we get

[0050]

[0051] Step 8) By combining formulas (12) and (15), the true stress and true strain at the stretching time t1 can be obtained. By taking different stretching times, the true stress and true strain at different stretching times can be obtained, and the true stress-true strain curve can be drawn.

[0052] Compared with the existing method, the beneficial effects of the present invention are:

[0053] The present invention establishes a relationship curve between the volume increment caused by the sample being immersed in a solution and the sample's descending distance or the sample's uniform descending time, finds the relationship between the cross-sectional area of ​​the sample before fracture and the slope of the curve, thereby obtaining the change in the cross-sectional area of ​​the sample during high-temperature stretching, avoiding the limitation that the traditional method determined according to the law of volume invariance can only handle uniform deformation. Regardless of whether the sample is uniformly deformed during the stretching process, the true stress of the sample during the stretching process can be accurately obtained, thereby obtaining an accurate true stress-strain curve.

[0054] The present invention analyzes the deformation characteristics of the material and finds the cross-sectional area of ​​the sample corresponding to the force value in the deformation process, so as to effectively obtain the true stress-strain curve of the material in the high-temperature stretching process. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figure 1 It is a schematic diagram of the relationship between the total volume V of the solution of the present invention and the sample immersed therein and the descending distance d of the sample;

[0056] Figure 2 It is a schematic diagram of the relationship between the total volume V of the solution of the present invention and the sample immersed therein and the sample falling time t;

[0057] Figure 3 Schematic diagram of the relationship between the total volume increment ΔV of the solution of the present invention and the sample immersed therein and the descending distance d of the sample;

[0058] Figure 4 It is a schematic diagram of a curve showing the relationship between the total volume increment ΔV of the solution of the present invention and the sample immersed therein and the sample falling time t;

[0059] Figure 5 is a graph showing the relationship between the total volume V of the solution and the sample immersed therein and the descending distance d of the sample measured in Examples 1 and 3 of the present invention;

[0060] Figure 6 is a graph showing the relationship between the total volume increment ΔV of the solution and the sample immersed therein and the descending distance d of the sample measured in Examples 1 and 3 of the present invention;

[0061] Figure 7 is a graph showing the relationship between the total volume V of the solution and the sample immersed therein and the sample falling time t measured in Examples 2 and 4 of the present invention;

[0062] Figure 8 is a relationship curve between the total volume increment ΔV of the solution and the part of the sample immersed in the solution and the falling time t of the sample measured in Examples 2 and 4 of the present invention;

[0063] Fig. 9 is the true stress-strain curve of the materials of Examples 1 and 3 of the present invention under high temperature stretching;

[0064] Fig.10 It is the true stress-strain curve of the materials of Examples 2 and 4 of the present invention under high temperature tensile test. DETAILED DESCRIPTION

[0065] The present invention discloses a test calculation method for obtaining a true stress-strain curve of high temperature tension. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters for implementation. It is particularly important to point out that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0066] A test calculation method for obtaining a high temperature tensile true stress-strain curve, the method specifically comprising the following steps:

[0067] 1. Obtain the sample through simulation experiment. Select a rod-shaped cylinder with a simulated sample length of L0, and use a thermal simulation test machine to heat, keep warm, and cool the simulated sample according to the predetermined experimental plan, and then stretch it at 600-1400℃, with a stretching rate of Vt, mm / s, until the sample is broken, and a sample broken into two sections is obtained.

[0068] Based on the deformation behavior of the sample at high temperature, the sample is broken into two sections, one end of each section near the fracture is in a table shape, and the rest is in a cylindrical shape. The two sections of the sample are butted together to form a whole, and the two sections of the sample can be joined to the state of the sample at the moment of stretching and breaking by magnetization or adhesion.

[0069] 2. Take a container with enough solution and place it on a horizontal surface. The solution does not react with the sample. Place the axis of the two connected sample sections in step 1 perpendicular to the liquid surface of the solution and slowly place it in the solution in a direction perpendicular to the liquid surface of the solution. There are two ways to place it: one is to drop the same distance d, mm each time; the other is to drop the sample at a uniform speed, with a drop speed of v d , mm / s.

[0070] When descending, record the rise of the solution level H, mm; the total volume of the solution and the sample immersed therein V, ml.

[0071] 3. Draw the relationship curve between the total volume V, ml of the solution and the sample immersed therein and the distance d of the sample falling, or the relationship curve between the total volume V, ml of the solution and the sample immersed therein and the time t of the sample falling, as shown in step 2. Figure 1 and 2 shown.

[0072] When the sample is just immersed in the solution, the sample causes the liquid level to rise, causing the volume of the solution to increase. The increase is the volume of the cylinder immersed in the solution. Since the cross section of the cylinder is equal everywhere, the curve rises in a straight line. When the table-shaped part of the sample is immersed in the solution, the cross section at this time gradually decreases as the sample descends, so the slope of the curve also decreases. When the sample continues to descend to another section, the cross section at this time gradually increases as the sample descends, so the slope of the curve also increases. Finally, the table-shaped part of the sample is completely immersed in the solution, and the increase in the volume of the solution is only affected by the volume of the cylinder immersed in the solution, and the curve rises in a straight line again.

[0073] 4. Based on the curve analysis drawn in step 3, the first-order differential of the curve is performed to obtain the relationship curve between the slope of the curve and the sample falling distance d or the slope of the curve and the sample falling time. The slope of the curve corresponds to the volume increment ΔV, ml, such as Figure 3 and 4 shown.

[0074] The maximum value of the curve corresponds to the maximum cross-sectional area of ​​the specimen S1, mm 2 , the minimum value of the curve corresponds to the minimum cross-sectional area of ​​the specimen S2, mm 2 The minimum cross-sectional area at the fracture of the specimen is S2. The distance the specimen drops from the maximum value to the minimum value of the curve is set to Δd, mm. If the drop time is set to Δt, s.

[0075] 5. The curve obtained according to step 4 Figure 3 and 4 , perform polynomial fitting on the part between the point where the curve starts to drop and the point where the curve drops to the lowest point, and obtain the relationship between the volume increment ΔV and the drop distance or drop time:

[0076] ΔV=f(d) (1)

[0077] ΔV=f(t) (2)

[0078] Figure 3 or Figure 4 The maximum value of the curve in corresponds to a volume increment of ΔV0, which corresponds to the maximum cross-sectional area S1 of the sample, that is, the original cross-sectional area of ​​the sample. Both parameters are known, and the ratio of the two is K.

[0079] but

[0080]

[0081] The volume increment ΔV is proportional to the cross-sectional area S of the sample, then

[0082]

[0083] Substituting formula (4) into formula (1) and formula (2), we get

[0084] S=f(d)K (5)

[0085] S=f(t)K (6)

[0086] The function of the cross-sectional area of ​​the specimen within the entire deformation region is established by equations (5) and (6).

[0087] 6. Assume that in step 1, the time taken for the sample to be stretched from the beginning to a certain length is t1, s, the tensile force at this time is F1, N, and the time taken for the sample to be stretched from the beginning to being broken is t0, s. If the cross-sectional area of ​​the sample after the stretching time t1 is calculated according to the sample's descending distance, then

[0088]

[0089] Substituting the above formula into formula (5), we get

[0090]

[0091] Among them, Δd, t0, and K are constants that can be measured experimentally;

[0092] If the cross-sectional area of ​​the sample after the sample stretching time t1 is calculated according to the sample falling time, then

[0093]

[0094] Substituting the above formula into formula (6), we get

[0095]

[0096] Among them, Δt, t0, K are constants and can be measured experimentally.

[0097] Formulas (8) and (12) are the relationship between the cross-sectional area of ​​the sample and the stretching time t1 during the stretching process under two methods. The relationship between the tensile force of the sample and the stretching time t1 during the stretching process can be obtained by collecting corresponding data from the testing machine, which is:

[0098] F1=g(t1) (11)

[0099] Then substitute formula (8) and (11) or (10) and (11) into the following formula:

[0100]

[0101] The relationship between the true stress and the stretching time during the deformation process of the sample is obtained.

[0102] 7. The relationship between true strain and engineering strain is:

[0103] ε=ln(1+e) (13)

[0104] Where ε is the true strain and e is the engineering strain

[0105] From step 1, the original length of the sample is L0, and the tensile rate is V t , mm / s, then

[0106]

[0107] Substituting formula (14) into formula (13), we get

[0108]

[0109] 8. Combining formulas (12) and (15), we can get the true stress and true strain at the stretching time t1. Taking different stretching times, we can get the true stress and true strain at different stretching times, and then draw the true stress-true strain curve.

[0110] [Example]

[0111] Embodiment 1: A test calculation method for obtaining a high temperature tensile true stress-strain curve, the method specifically comprising the following steps:

[0112] Step 1: Obtain the sample through simulation experiment. The material is a low-carbon steel, which is processed into a simulation sample with a size of Φ10×125mm cylinder. It is heated to 1300℃ by a thermal simulation test machine, kept warm for 5 minutes, then cooled to 1000℃ at a rate of 3℃ / s, and then kept warm for 1 minute for stretching. The stretching rate is set to 6×10 -2 mm / s until the sample is broken and a sample is obtained. Based on the deformation behavior of the sample at high temperature, the sample is broken into two sections, one end of each section near the fracture is in a table shape, and the rest is in a cylindrical shape. The two sections of the sample are magnetized and butted together to form a whole.

[0113] Step 2: Take a container filled with sufficient water and place it on a horizontal surface. Place the axis of the two sections of the sample that have been connected in step 1 perpendicular to the water surface and slowly place them in the solution. During the placement process, lower them by the same distance of 0.5 mm each time.

[0114] Step 3: Draw a curve of the relationship between the total volume of water and the part of the sample immersed in water and the distance the sample falls in step 2, such as Figure 5 shown.

[0115] Step 4: Based on the curve analysis drawn in step 3, the first-order differential of the curve is performed to obtain the relationship curve of the slope of the curve as the sample descends the distance d, such as Figure 6The maximum slope K1 of the curve corresponds to the maximum cross-sectional area S1 of the sample, the minimum slope K2 of the curve corresponds to the minimum cross-sectional area S2 of the sample, and the distance the sample drops from the maximum value to the minimum value is 7.75 mm;

[0116] Step 5: For the curve obtained in step 4 Figure 6 Analysis, a trinomial fitting is performed on the part between the point where the curve starts to drop and the point where the curve drops to the lowest point in the figure, and the relationship between the volume increment ΔV and the drop distance is obtained as follows:

[0117] ΔV=115.3-5.78d-0.70d 2 +0.046d 3 (16)

[0118] Figure 6 The maximum value of the curve in corresponds to a volume increment of 78.5 mm 3 , corresponding to the maximum cross-sectional area of ​​the specimen 78.5mm 2 , that is, the original cross-sectional area of ​​the specimen. From formula (3), we get the ratio of the two, K = 1 mm. Substituting formula (4) into (16), we get

[0119] S=115.3-5.78d-0.70d 2 +0.046d 3 (17)

[0120] The function of the cross-sectional area of ​​the specimen within the entire deformation region is established by formula (17).

[0121] Step 6: The time taken for the sample to be stretched from the beginning to the breaking is 76 s. According to formula (7),

[0122]

[0123] Substituting the above formula into formula (17) we get

[0124]

[0125] Step 7: The area calculated by formula (19) is matched with the tension collected by the equipment at the same time, formula (11), and the true stress value is calculated according to formula (12). Then the obtained value is matched with the true strain obtained by formulas (13), (14) and (15) to obtain the true stress-strain curve, as shown in Fig. 9 shown.

[0126] Embodiment 2: A test calculation method for obtaining a high temperature tensile true stress-strain curve, the method specifically comprising the following steps:

[0127] Step 1: Obtain the sample through simulation experiment. The material is a low-carbon steel, which is processed into a simulation sample with a size of Φ10×125mm cylinder. It is heated to 1300℃ by a thermal simulation test machine, kept warm for 5 minutes, then cooled to 1000℃ at a rate of 3℃ / s, and then kept warm for 1 minute for stretching. The stretching rate is set to 6×10 -2 mm / s until the sample is broken and a sample is obtained. Based on the deformation behavior of the sample at high temperature, the sample is broken into two sections, one end of each section near the fracture is in a table shape, and the rest is in a cylindrical shape. The two sections of the sample are magnetized and butted together to form a whole.

[0128] Step 2: Take a container with sufficient water and place it on a horizontal surface. Place the two sections of the sample connected in step 1 with their axes perpendicular to the water surface and slowly place them in the solution. During the placement process, the sample descends at a constant speed, with a descending speed of v = 1 mm / s.

[0129] Step 3: Draw a curve of the relationship between the total volume of water and the part of the sample immersed in water and the sample descent time in step 2, such as Figure 7 shown.

[0130] Step 4: Based on the curve analysis drawn in step 3, the curve is differentiated in the first order to obtain the relationship curve between the slope of the curve and the falling time of the sample, such as Figure 8 The maximum slope K1 of the curve corresponds to the maximum cross-sectional area S1 of the sample, the minimum slope K2 of the curve corresponds to the minimum cross-sectional area S2 of the sample, and the sample falling time from the maximum value to the minimum value is 7.76s.

[0131] Step 5: For the curve obtained in step 4 Figure 8 Analysis, a trinomial fitting is performed on the part between the point where the curve starts to drop and the point where the curve drops to the lowest point in the figure, and the relationship between the volume increment ΔV and the drop time is obtained as follows:

[0132] ΔV=113.6-5.07t-0.79t 2 +0.05t 3 (20)

[0133] Figure 8 The maximum value of the curve in corresponds to a volume increment of 78.5 mm 3 , corresponding to the maximum cross-sectional area of ​​the specimen 78.5mm 2 , that is, the original cross-sectional area of ​​the specimen. From formula (3), we get the ratio of the two, K = 1 mm. Substituting formula (4) into (16), we get

[0134] S=113.6-5.07t-0.79t 2 +0.05t 3 (twenty one)

[0135] The function of the cross-sectional area of ​​the specimen within the entire deformation region is established by formula (21).

[0136] Step 6: The time taken for the sample to be stretched from the beginning to the breaking is 76 s. According to formula (9),

[0137]

[0138] Substituting the above formula into formula (21), we get

[0139]

[0140] Step 7: The area calculated by formula (23) is matched with the tension collected by the equipment at the same time, formula (11), and the true stress value is calculated according to formula (12). Then, the obtained value is matched with the true strain obtained by formulas (13), (14) and (15) to obtain the true stress-strain curve, as shown in Fig.10 shown.

[0141] Embodiment 3:

[0142] Step 1: Obtain the sample through simulation experiment. The material is a low-carbon steel, which is processed into a simulation sample with a size of Φ10×125mm cylinder. It is heated to 1300℃ by a thermal simulation test machine, kept warm for 5 minutes, then cooled to 700℃ at a rate of 3℃ / s, and then kept warm for 1 minute for stretching. The stretching rate is set to 6×10 -2 mm / s until the sample is broken and a sample is obtained. Based on the deformation behavior of the sample at high temperature, the sample is broken into two sections, one end of each section near the fracture is in a table shape, and the rest is in a cylindrical shape. The two sections of the sample are magnetized and butted together to form a whole.

[0143] Step 2: Take a container filled with sufficient water and place it on a horizontal surface. Place the axis of the two sections of the sample connected in step 1 perpendicular to the water surface and slowly place them in the solution. During the placement process, lower them by the same distance of 0.5 mm each time.

[0144] Step 3: Draw a curve of the relationship between the total volume of water and the part of the sample immersed in water and the distance the sample falls in step 2, such as Figure 5 shown.

[0145] Step 4: Based on the curve analysis drawn in step 3, the first-order differential of the curve is performed to obtain the relationship curve of the slope of the curve as the sample descends the distance d, such as Figure 6 The maximum slope K1 of the curve corresponds to the maximum cross-sectional area S1 of the sample, the minimum slope K2 of the curve corresponds to the minimum cross-sectional area S2 of the sample, and the sample drops 5.15 mm from the maximum value to the minimum value.

[0146] Step 5: Analyze the curve obtained in step 4, perform trinomial fitting on the portion between the starting point of the curve and the lowest point of the curve, and obtain the relationship between the volume increment ΔV and the descending distance as follows:

[0147] ΔV=95.3-7.32d-0.56d 2 +0.061d 3 (twenty four)

[0148] The maximum value of the curve corresponds to a volume increment of 78.5 mm 3 , corresponding to the maximum cross-sectional area of ​​the specimen 78.5mm 2 , that is, the original cross-sectional area of ​​the specimen. From formula (3), we get the ratio of the two, K = 1 mm. Substituting formula (4) into (24), we get

[0149] S=95.3-7.32d-0.56d 2 +0.061d 3 (25)

[0150] The function of the cross-sectional area of ​​the specimen in the entire deformation region is established by formula (25);

[0151] Step 6: The time taken for the sample to be stretched from the beginning to the breaking is 56 s. According to formula (7),

[0152]

[0153] Substituting the above formula into formula (25) we get

[0154]

[0155] Step 7: The area calculated by formula (27) is matched with the tension collected by the equipment at the same time, formula (11), and the true stress value is calculated according to formula (12). Then, the obtained value is matched with the true strain obtained by formulas (13), (14) and (15) to obtain the true stress-strain curve, as shown in Fig. 9 shown.

[0156] Embodiment 4:

[0157] Step 1: Obtain the sample through simulation experiment. The material is a low-carbon steel, which is processed into a simulation sample with a size of Φ10×125mm cylinder. It is heated to 1300℃ by a thermal simulation test machine, kept warm for 5 minutes, then cooled to 700℃ at a rate of 3℃ / s, and then kept warm for 1 minute for stretching. The stretching rate is set to 6×10 -2mm / s until the sample is broken and a sample is obtained. Based on the deformation behavior of the sample at high temperature, the sample is broken into two sections, one end of each section near the fracture is in a table shape, and the rest is in a cylindrical shape. The two sections of the sample are magnetized and butted together to form a whole.

[0158] Step 2: Take a container with sufficient water and place it on a horizontal surface. Place the two sections of the sample connected in step 1 with their axes perpendicular to the water surface and slowly place them in the solution. During the placement process, the sample descends at a constant speed, with a descending speed of v = 1 mm / s.

[0159] Step 3: Draw a curve of the relationship between the total volume of water and the part of the sample immersed in water and the sample descent time in step 2, such as Figure 7 shown.

[0160] Step 4: Based on the curve analysis drawn in step 3, the curve is differentiated in the first order to obtain the relationship curve between the slope of the curve and the falling time of the sample, such as Figure 8 The maximum slope K1 of the curve corresponds to the maximum cross-sectional area S1 of the sample, the minimum slope K2 of the curve corresponds to the minimum cross-sectional area S2 of the sample, and the sample falling time from the maximum value to the minimum value is 5.15s.

[0161] Step 5: Analyze the curve graph obtained in step 4, perform trinomial fitting on the portion between the point where the curve starts to decline and the point where the curve drops to the lowest point, and obtain the relationship between the volume increment ΔV and the decline time as follows:

[0162] ΔV=92.1-4.27t-1.06t 2 +0.039t 3 (28)

[0163] Figure 8 The maximum value of the curve in corresponds to a volume increment of 78.5 mm 3 , corresponding to the maximum cross-sectional area of ​​the specimen 78.5mm 2 , that is, the original cross-sectional area of ​​the specimen. From formula (3), we get the ratio of the two, K = 1 mm. Substituting formula (4) into (28), we get

[0164] S=92.1-4.27t-1.06t 2 +0.039t 3 (29)

[0165] The function of the cross-sectional area of ​​the specimen in the entire deformation region is established by formula (29);

[0166] Step 6: The time taken for the sample to be stretched from the beginning to the breaking is 56 s. According to formula (9),

[0167]

[0168] Substituting the above formula into formula (29) we get

[0169]

[0170] Step 7: The area calculated by formula (31) is matched with the tension collected by the equipment at the same time, formula (11), and the true stress value is calculated according to formula (12). Then, the obtained value is matched with the true strain obtained by formulas (13), (14) and (15) to obtain the true stress-strain curve, as shown in Fig.10 shown.

[0171] The present invention establishes a relationship curve between the volume increment caused by the sample being immersed in a solution and the sample's descending distance or the sample's uniform descending time, and finds the relationship between the cross-sectional area of ​​the sample before fracture and the slope of the curve, thereby obtaining the change in the cross-sectional area of ​​the sample during the high-temperature stretching process. Regardless of whether the sample is deformed uniformly during the stretching process, the true stress of the sample during the stretching process can be accurately obtained, thereby obtaining an accurate true stress-strain curve.

[0172] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A test calculation method for obtaining a high temperature tensile true stress-strain curve, characterized in that: The method specifically comprises the following steps: Step 1) A cylindrical rod-shaped specimen with a length of L0, mm is selected, and the simulated specimen is heated, kept warm, cooled, and then stretched by a thermal simulation test machine according to a predetermined experimental plan, and the stretching rate is v t , mm / s, until the sample is broken and a sample broken into two sections is obtained; The two sections of the specimen are butt-joined to form a coaxial whole, and the two sections of the specimen are joined to the state at the moment of the specimen being stretched and broken; Step 2) using a solution that does not react with the sample, injecting the solution into a container, placing the container on a horizontal surface, and placing the sample in the solution along a direction perpendicular to the liquid surface of the solution with the axis of the sample after docking perpendicular to the liquid surface of the solution; During the insertion process, the same distance d, mm, is dropped each time; When descending, record the rise of the solution level H, mm; the total volume of the solution and the sample immersed therein V, ml; Step 3) drawing a relationship curve between the total volume V, ml, of the solution and the sample immersed therein and the distance d from which the sample descends; Step 4) taking the first-order differential of the curve, the slope of the curve is obtained as the sample descends by a distance d, and the slope of the curve corresponds to the volume increment ΔV, ml; The maximum value of the curve corresponds to the maximum cross-sectional area of ​​the specimen S1, mm 2 , the minimum value of the curve corresponds to the minimum cross-sectional area of ​​the specimen S2, mm 2 The minimum cross-sectional area at the fracture of the specimen is S2, and the distance the curve drops from the maximum value to the minimum value of the specimen is set as Δd, mm; Step 5) Perform polynomial fitting on the portion between the point where the curve starts to drop and the point where the curve drops to the lowest point, and obtain the relationship between the volume increment ΔV and the drop distance d as follows: ΔV=f(d)(1) The maximum value of the curve corresponds to a volume increment of ΔV0, which corresponds to the maximum cross-sectional area S1 of the sample, that is, the original cross-sectional area of ​​the sample. These two parameters are known. Assuming the ratio of the two is K, then The volume increment ΔV is proportional to the cross-sectional area S of the sample, then Substituting formula (4) into formula (1), we get S=f(d) / K (5) The function of the cross-sectional area of ​​the specimen in the entire deformation region is established by formula (5); Step 6) Assume that when performing step 1), the time taken for the sample to be stretched from the beginning to a certain length is t1, s, the tensile force value at this time is F1, N, and the time taken for the sample to be stretched from the beginning to being broken is t0, s. If the cross-sectional area of ​​the sample after the stretching time t1 is calculated according to the sample's descending distance, then Substituting the above formula into formula (5), we get Among them, Δd, t0, and K are constants measured by experiments; Formula (8) is the relationship between the cross-sectional area of ​​the sample and the stretching time during the stretching process, and the relationship between the tensile force of the sample and the stretching time t1 during the stretching process, which is obtained by collecting the corresponding data from the testing machine: F1=g(t1) (11) Substituting formula (8) and (11) into the following formula Obtain the relationship between the true stress and the stretching time during the deformation process of the sample; Step 7) The relationship between true strain and engineering strain is: ε=ln(1+e) (13) Where ε is the true strain and e is the engineering strain From step 1, the original length of the sample is L0, and the tensile rate is V t , mm / s, then Substituting formula (14) into formula (13), we get Step 8) Combine formulas (12) and (15) to obtain the true stress and true strain at the stretching time t1. Take different stretching times to obtain the true stress and true strain at different stretching times, and draw the true stress-true strain curve.

2. A test calculation method for obtaining a high temperature tensile true stress-strain curve according to claim 1, characterized in that: In the step 1), two sections of the sample are joined together by magnetization or adhesion to form a state at the moment when the sample is stretched and broken.

3. A test calculation method for obtaining a high temperature tensile true stress-strain curve according to claim 1, characterized in that: In the step 2), during the placement process, the sample descends at a constant speed, and the descending speed is v d , mm / s; Step 3) drawing a relationship curve between the total volume V, ml of the solution and the sample immersed therein and the sample falling time t; Step 4) performing first-order differentiation on the curve to obtain a curve showing the relationship between the slope of the curve and the falling time of the sample, wherein the slope of the curve corresponds to the volume increment ΔV, ml; The maximum value of the curve corresponds to the maximum cross-sectional area of ​​the specimen S1, mm 2 , the minimum value of the curve corresponds to the minimum cross-sectional area of ​​the specimen S2, mm 2 The minimum cross-sectional area at the fracture of the specimen is S2, and the time for the specimen to fall from the maximum value to the minimum value of the curve is Δt, s; Step 5) Perform polynomial fitting on the portion between the point where the curve starts to decline and the point where the curve drops to the lowest point, and obtain the relationship between the volume increment ΔV and the decline time as follows: ΔV=f(t)(2) The maximum value of the curve corresponds to a volume increment of ΔV0, which corresponds to the maximum cross-sectional area S1 of the sample, that is, the original cross-sectional area of ​​the sample. These two parameters are known. Assuming the ratio of the two is K, then The volume increment ΔV is proportional to the cross-sectional area S of the sample, then Substituting formula (4) into formula (2), we get S=f(t) / K (6) The function of the cross-sectional area of ​​the specimen in the entire deformation region is established by formula (6); Step 6) Assume that when performing step 1), the time taken for the sample to be stretched from the beginning to a certain length is t1, s, the tensile force value at this time is F1, N, and the time taken for the sample to be stretched from the beginning to being broken is t0, s. Calculate the cross-sectional area of ​​the sample after the sample is stretched for time t1 according to the sample descent time, then Substituting the above formula into formula (6), we get Among them, Δt, t0, and K are constants that can be measured experimentally; Formula (10) is the relationship between the cross-sectional area of ​​the sample and the stretching time t1 during the stretching process. The relationship between the tensile force of the sample and the stretching time t1 during the stretching process can be obtained by collecting the corresponding data from the testing machine, which is: F1=g(t1) (11) Substitute formulas (10) and (11) into the following formula: The relationship between the true stress and the stretching time during the deformation process of the sample is obtained.

4. A test calculation method for obtaining a high temperature tensile true stress-strain curve according to claim 1, characterized in that: In the step 3), when the sample is just immersed in the solution, the curve rises linearly; when the table-shaped part of the sample is immersed in the solution, the slope of the curve decreases; when the sample continues to descend to another section, the slope of the curve increases; finally, the curve rises linearly again.

Citation Information

Patent Citations

  • Single-shaft tensile overall true stress-true strain curve testing technique

    CN102221503A

  • Determination of turbine blade cross-sectional area

    CN1035157A

  • Method for testing true stress and true strain of metal material

    CN107271279A

  • Obtaining method of high temperature tensile test true stress

    CN108489820A

  • True stress-true strain curve test calculation method based on digital image correlation method

    CN112927185A